Metal Oxide Varistor: Zinc Oxide with Bismuth and Aluminium Oxides, 1350 °C (Masuyama 1972)

Masuyama, Matsuoka and Nishi found that adding a second oxide to zinc oxide and bismuth oxide changes the varistor a great deal. This is their Example 2 with aluminium oxide: 99.0 % zinc oxide, 0.5 % bismuth oxide and 0.5 % aluminium oxide by moles, sintered at 1350 °C. The disc measured a C-value of 3.6 at 1 mA and a nonlinearity exponent n of 4.6. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 2. Unknown: how the aluminium is sprayed on and what the silver paint is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Erfahren
1 day

Anweisungen

1

Weigh 99.0 : 0.5 : 0.5 and wet-mill 5 hours

Mix zinc oxide, bismuth oxide and aluminium oxide 99.0 : 0.5 : 0.5 by moles. Ours, for 10 g: 9.66 g zinc oxide, 0.279 g bismuth oxide, 0.061 g aluminium oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.

Materialien für diesen Schritt:

ZinkoxidpulverZinkoxidpulver9.66 g
BismutoxidBismutoxid0.279 g
Tonerdepulver (Aluminiumoxid)Tonerdepulver (Aluminiumoxid)0.061 g

Benötigte Werkzeuge:

BalkenwaageBalkenwaage
EisenkugelmühleEisenkugelmühle
TrockenofenTrockenofen
2

Press discs 13 mm by 2.5 mm

Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.

Benötigte Werkzeuge:

Hydraulische PresseHydraulische Presse
Scheiben-PressformScheiben-Pressform
MessschieberMessschieber
3

Sinter 1 hour at 1350 °C and furnace-cool

Sinter the discs in air at 1350 °C for 1 hour, then let them cool in the furnace to room temperature (about 15-30 °C).

Benötigte Werkzeuge:

MuffelofenMuffelofen
4

Lap to 10 mm by 1.5 mm

Lap both faces with 600-mesh silicon carbide. The finished disc is 10 mm across and 1.5 mm thick.

Benötigte Werkzeuge:

Siliciumcarbid-KörnungSiliciumcarbid-Körnung
MessschieberMessschieber
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.

Materialien für diesen Schritt:

AluminiumbarrenAluminiumbarren1 as required
SilberleitlackSilberleitlack1 as required
KupferdrahtKupferdraht2 Stück

Benötigte Werkzeuge:

Unbekanntes MetallspritzverfahrenUnbekanntes Metallspritzverfahren
MessschieberMessschieber

Materialien

6

Benötigte Werkzeuge

9

Verwandte Blueprints

Diese Blueprints teilen Wissen — Techniken, Materialien oder Prinzipien

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...