Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)
Charlie

Creado por

Charlie

28. octubre 2026DE
4
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)

A ceramic magnet with a fifth of the barium replaced by calcium: 0.08 mol barium carbonate, 0.02 mol calcium carbonate and 0.6 mol iron oxide, made as in Example 18 but sintered at 1290 °C for only 5 minutes. Went's rod held 1,615 gauss with a coercive force of 1,550 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 20. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
2 days

Instrucciones

1

Weigh barium carbonate, chalk and iron oxide

Weigh 15.79 g barium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiales para este paso:

Carbonato de bario (witherita)Carbonato de bario (witherita)15.79 g
Carbonato de calcio (blanco de España)Carbonato de calcio (blanco de España)2.002 g
Óxido férricoÓxido férrico95.55 g

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Guantes de gomaGuantes de goma
Respirador P100Respirador P100
2

Mill, presinter and mill as in Example 18

As in Example 18: grind with alcohol 4 hours, dry at 150 °C, fire in air at 1000 °C for 2 hours, grind again 4 hours and dry.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
Horno muflaHorno mufla
Crisol con tapa (porcelana)Crisol con tapa (porcelana)
Tenazas para crisolTenazas para crisol
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm², as in Example 18 (ours: discs instead of rods).

Herramientas necesarias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
4

Pass through a 1290 °C zone in 5 minutes

Sinter in air at 1290 °C by passing the pieces through a 10 cm hot zone at 20 mm per minute: 5 minutes in the heat.

Herramientas necesarias:

Horno tubularHorno tubular
Guantes resistentes al calorGuantes resistentes al calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Herramientas necesarias:

ElectroimánElectroimán
BrújulaBrújula

Materiales

3

Herramientas requeridas

15

Blueprints relacionados

Estos blueprints comparten conocimiento — técnicas, materiales o principios

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...