Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)

A barium ferrite made with more iron oxide, 0.4 mol barium carbonate to 3.6 mol, fired an hour at 1300 °C in carbon dioxide. Little oxygen gives the hexagonal crystal BaFe18O27, with some iron in the lower state. It is milled again, bound with nitrocellulose or polyvinyl alcohol, and pressed hard at 12 tonnes per cm². Went's rod held 1,260 gauss with a coercive force of 700 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 33. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
2 days

Instrucciones

1

Weigh barium carbonate and iron oxide

Weigh 79.4 g barium carbonate (0.4 mol) and 580.9 g ferric oxide (3.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiales para este paso:

Carbonato de bario (witherita)Carbonato de bario (witherita)79.4 g
Óxido férricoÓxido férrico580.9 g

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Guantes de gomaGuantes de goma
Respirador P100Respirador P100
2

Mill 15.5 hours, press a pastille, fire in CO2

Grind with alcohol in a ball mill for 15.5 hours, dry, and press into a pastille. Heat it at 1300 °C in carbon dioxide for 1 hour (ours: a tube furnace fed from a CO2 cylinder).

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
Horno tubularHorno tubular
Dióxido de carbono gaseosoDióxido de carbono gaseoso
Bombona de gas a presiónBombona de gas a presión
Guantes resistentes al calorGuantes resistentes al calor
3

Pulverise, mill 14 hours, bind

Crush the cooled pastille and grind it with alcohol for 14 hours. Press the powder into a pastille again with a ceramic binder (ours: polyvinyl alcohol, one of the two named), then crush it to grains.

Materiales para este paso:

Alcohol polivinílico en polvoAlcohol polivinílico en polvo1 as required

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
4

Press at 12 tonnes per cm²

Press the grains at 12 tonnes per cm² (ours: discs instead of rods). The patent describes no further firing.

Herramientas necesarias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Herramientas necesarias:

ElectroimánElectroimán
BrújulaBrújula

Materiales

3

Herramientas requeridas

14

Blueprints relacionados

Estos blueprints comparten conocimiento — técnicas, materiales o principios

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...