Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)
Charlie

Creado por

Charlie

28. octubre 2026DE
6
0
0
0
0

Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)

A barium ferrite with much more iron oxide: 0.5 mol barium carbonate to 3.5 mol, milled 15.5 hours, bound, formed and sintered 10 minutes at 1330 °C. Went's rod held 2,040 gauss with a coercive force of 2,380 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 4. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
2 days

Instrucciones

1

Weigh barium carbonate and iron oxide

Weigh 99.2 g barium carbonate (0.5 mol) and 564.8 g ferric oxide (3.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiales para este paso:

Carbonato de bario (witherita)Carbonato de bario (witherita)99.2 g
Óxido férricoÓxido férrico564.8 g

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Guantes de gomaGuantes de goma
Respirador P100Respirador P100
2

Mill with alcohol 15.5 hours, dry and sieve

Grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
CribaCriba
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Herramientas necesarias:

Alcohol polivinílico en polvoAlcohol polivinílico en polvo
Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
Horno de secadoHorno de secado
4

Sinter in air at 1330 °C for 10 minutes

Sinter the pieces in air at 1330 °C for 10 minutes. The patent gives no zone length or speed for this example.

Herramientas necesarias:

Horno tubularHorno tubular
Guantes resistentes al calorGuantes resistentes al calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Herramientas necesarias:

ElectroimánElectroimán
BrújulaBrújula

Materiales

2

Herramientas requeridas

14

Blueprints relacionados

Estos blueprints comparten conocimiento — técnicas, materiales o principios

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.