Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate
Forge

Creado por

Forge

18. octubre 2026NO
14
0
0
0
0

Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate

Bearing balls are headed from thick wire of 52100 steel. Here 52100 bar is forged to rod and drawn through a drawplate. At 1 % carbon it is much harder than mild steel, so it is annealed soft before drawing and again after every two holes, using the 52100 anneal Verhoeven recommends. The picture: our drawing, bar to coil.
Avanzado
2 days

Instrucciones

1

Forge to rod

Heat the bar to a cherry-red heat and no hotter, and draw it out round on the anvil to a rod a little thicker than the drawplate's largest hole.

Materiales para este paso:

Barra de acero para rodamientos (52100)Barra de acero para rodamientos (52100)1 kg
Carbón vegetalCarbón vegetal1 as required

Herramientas necesarias:

Fragua de herreroFragua de herrero
YunqueYunque
Martillo de peña transversalMartillo de peña transversal
Tenazas de herreroTenazas de herrero
Guantes de soldadorGuantes de soldador
Gafas de seguridadGafas de seguridad
2

Anneal

In the oven, hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Herramientas necesarias:

Horno de tratamiento térmicoHorno de tratamiento térmico
Termopar con indicadorTermopar con indicador
Tenazas de herreroTenazas de herrero
Guantes de soldadorGuantes de soldador
3

Clean and taper

Brush off all the scale, then file a long taper on the first 3 cm so it passes the first hole.

Herramientas necesarias:

Juego de cepillos de alambreJuego de cepillos de alambre
Juego de limasJuego de limas
Tornillo de bancoTornillo de banco
4

Wax and draw

Clamp the drawplate in the vise. Wax the rod, push the taper through the first hole it does not slip through, and pull straight out with the draw tongs in one steady pull.

Materiales para este paso:

Cera de abejaCera de abeja20 g

Herramientas necesarias:

Hilera de aceroHilera de acero
Tenazas de estirarTenazas de estirar
Tornillo de bancoTornillo de banco
Guantes de trabajo de cueroGuantes de trabajo de cuero
5

Anneal every two holes

Draw through each next hole without skipping. After every two holes, coil the wire and anneal it again: hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Materiales para este paso:

Cera de abejaCera de abeja1 pieza

Herramientas necesarias:

Hilera de aceroHilera de acero
Tenazas de estirarTenazas de estirar
Horno de tratamiento térmicoHorno de tratamiento térmico
Termopar con indicadorTermopar con indicador
6

Finish soft

Stop at the diameter your balls need, checked with the caliper, and give the coil a last anneal so it is soft for heading.

Herramientas necesarias:

Calibre digital de 6 pulgadasCalibre digital de 6 pulgadas
Horno de tratamiento térmicoHorno de tratamiento térmico
Termopar con indicadorTermopar con indicador
7

Troubleshooting

Bearing steel wire troubleshooting.

Flow

Loading...

Materiales

3

Herramientas requeridas

15

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...