Smith's Fire Rake (Poker): a 3/8 in. Rod Drawn to a Flat Point, Crooked, and Looped Over the Anvil (Edwinson, 1886)
Forge

Creado por

Forge

14. noviembre 2026NO
8
0
0
0
0

Smith's Fire Rake (Poker): a 3/8 in. Rod Drawn to a Flat Point, Crooked, and Looped Over the Anvil (Edwinson, 1886)

The first job George Edwinson set his readers in Amateur Work (1886): the smith's rake for the forge fire, which "might be dubbed a poker". A yard of 3/8 in. iron rod drawn to a square then flat point with quarter turns, bent into a crook, and the other end bent round in three heats into a loop handle.
Principiante
An hour at the forge

Instrucciones

1

His sizes

Cargando el cuaderno de Jupyter…
2

Read Edwinson

"The rake, Fig. 16, might be dubbed a poker, and as this is the most simple tool, we will deal with that first."
3

Light a small fire

Pile slack round the tuyere, scoop a shallow pit in front of it, put in shavings with a few cinders on top, light and blow gently. Draw slack in until the heap glows, then damp the outside so the fire stays within 6 in. (15 cm) of the tuyere.

Materiales para este paso:

Carbón bituminosoCarbón bituminoso1 pieza

Herramientas necesarias:

Fragua de herreroFragua de herrero
4

Draw the point

Cut 36 in. (91 cm) of 3/8 in. (10 mm) iron rod with a cold chisel. Heat 2 in. of one end glowing white. On the outer edge of the anvil, hammer it lightly on the tip, giving the rod a quarter turn after each blow and drawing it back, to a square point. Strike only while it glows; reheat at a dull red. Next heat, round the corners and draw a flat tapering point (fig. 17).

Materiales para este paso:

Barra de hierro forjadoBarra de hierro forjado1 pieza

Herramientas necesarias:

CortafríosCortafríos
Fragua de herreroFragua de herrero
YunqueYunque
MartilloMartillo
5

Crook the end

Heat the point to a dull red and bend it over the outer edge of the anvil with a few light blows into the crook (fig. 16).

Herramientas necesarias:

Fragua de herreroFragua de herrero
YunqueYunque
MartilloMartillo
6

Bend the loop

Heat the rod about 10 in. from the other end to redness and bend it over the anvil edge (fig. 18). Heat 3 in. more of the bent part and shape it (fig. 19). Heat again and bring the end round to touch the shoulder (fig. 20), then shape the loop hot with light blows. (Experienced smiths scarf the end and weld it to the shoulder.)

Herramientas necesarias:

Fragua de herreroFragua de herrero
YunqueYunque
MartilloMartillo
7

Troubleshooting

Rake troubleshooting.

Flow

Loading...
8

History and honest limits

From George Edwinson, "Smithing and Forging" II, **Amateur Work, Illustrated**, vol. V (1886), pp. 211-213 and figs. 15-20 (checked on the archive.org scan amateurworkillus05lond). Metric figures and the tools are ours.

Materiales

2

Herramientas requeridas

4

Blueprints relacionados

Estos blueprints comparten conocimiento — técnicas, materiales o principios

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.