Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)
Charlie

Creado por

Charlie

28. octubre 2026DE
9
0
0
0
0

Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)

Extruded polystyrene foam blown with a butylene gas fraction. 300 lb of polystyrene and about 130 lb of the fraction stand two days at 110 °C under 265 psi. Opened again and again, the tower let out foam logs 20 inches across and 20 feet long, weighing only 0.8 lb per cubic foot. Unknown: a source for the butylene fraction, linked to an unknown head. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 4. Picture: the patent's drawing.
Avanzado
3 days

Instrucciones

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Materiales para este paso:

PoliestirenoPoliestireno300 libras

Herramientas necesarias:

Reactor a presiónReactor a presión
Balanza de platillosBalanza de platillos
Guantes de gomaGuantes de goma
2

Add the butylene fraction

Add about 130 lb of a cracked-oil gas fraction that is about 87 % normal butylenes, with some butanes and butadiene, under pressure. Unknown: a source for this fraction. Flammable gas: no flames, strong ventilation.

Materiales para este paso:

Fracción de gas de craqueo de butilenosFracción de gas de craqueo de butilenos130 libras

Herramientas necesarias:

Bombona de gas a presiónBombona de gas a presión
Reactor a presiónReactor a presión
Gafas de protección químicaGafas de protección química
3

Heat two days at 110 °C

Close the tower and heat it at 110 °C for two days. The gauge pressure stays at 265 psi.

Herramientas necesarias:

Reactor a presiónReactor a presión
Termómetro de laboratorioTermómetro de laboratorio
4

Let out logs through a 3.25 inch outlet

Open and close the 3.25 inch outlet near the bottom again and again. Each portion swells into a foam log 20 inches across and about 20 feet long, with fine, even, closed cells, weighing 0.8 lb per cubic foot.

Herramientas necesarias:

Reactor a presiónReactor a presión
Gafas de protección químicaGafas de protección química
Guantes de gomaGuantes de goma
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Herramientas necesarias:

Serrucho de carpinteroSerrucho de carpintero
Guantes de gomaGuantes de goma

Materiales

2

Herramientas requeridas

7

Blueprints relacionados

Estos blueprints comparten conocimiento — técnicas, materiales o principios

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...