Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 75 °C (McIntire, Dow 1948, Ex. 3, Test 4)
Charlie

Creado por

Charlie

28. octubre 2026DE
9
0
0
0
0

Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 75 °C (McIntire, Dow 1948, Ex. 3, Test 4)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 75 °C (395 psi in the tower), it swelled into a log 18 to 20 inches across, weighing 2.9 lb per cubic foot, with uniform cells finer than at 60 °C. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Avanzado
3 days

Instrucciones

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Materiales para este paso:

PoliestirenoPoliestireno300 libras

Herramientas necesarias:

Reactor a presiónReactor a presión
Balanza de platillosBalanza de platillos
Guantes de gomaGuantes de goma
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Materiales para este paso:

PropilenoPropileno100 libras

Herramientas necesarias:

Bombona de gas a presiónBombona de gas a presión
Reactor a presiónReactor a presión
Gafas de protección químicaGafas de protección química
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Herramientas necesarias:

Reactor a presiónReactor a presión
Termómetro de laboratorioTermómetro de laboratorio
4

Let it out at 75 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 75 °C. The pressure is about 395 psi. The gel flows out and swells into a log 18 to 20 inches across, 2.9 lb per cubic foot, with uniform cells finer than at 60 °C. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Herramientas necesarias:

Reactor a presiónReactor a presión
Termómetro de laboratorioTermómetro de laboratorio
Gafas de protección químicaGafas de protección química
Guantes de gomaGuantes de goma
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Herramientas necesarias:

Serrucho de carpinteroSerrucho de carpintero
Guantes de gomaGuantes de goma

Materiales

2
  • 300 libras
    Marcador de posición
  • 100 libras
    Marcador de posición

Herramientas requeridas

7

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...