Ferrite Toroid Core: Copper-Zinc Ferrite by the Wet Process, Precipitated with Caustic Soda (Snoek 1948)
Snoek's copper-zinc ferrite made the wet way: copper, zinc and iron salts thrown down together with hot caustic soda, so the particles are very fine and pure. The washed deposit is pre-heated, pressed into a ring and fired in oxygen, with a 30-hour hold at 600 °C. His core reached an initial permeability of 500.
Source: J. L. Snoek, US 2,452,529 (Philips, 1948), Example II, wet process. Picture: our diagram.
Avanzado
3 days
Instrucciones
1
1
Dissolve the copper, zinc and iron salts
Dissolve the copper, zinc and iron salts
Make 1 litre of a purified solution of 0.2 mol copper sulphate, 0.3 mol zinc sulphate and 1 mol iron nitrate. Ours: 49.94 g copper sulphate pentahydrate; weigh the zinc sulphate and ferric nitrate for the hydrate you have.
Materiales para este paso:
Sulfato de cobre pentahidratado (CuSO4·5H2O)49.94 g
Sulfato de zinc0.3 mol
Nitrato férrico1 mol
Agua destilada1 lHerramientas necesarias:
Balanza de platillos
Vaso de precipitados de borosilicato
Guantes de goma2
2
Precipitate hot with 9 M caustic soda
Precipitate hot with 9 M caustic soda
Heat the solution and precipitate it with 0.5 litre of 9 molar caustic soda. Ours: 180 g sodium hydroxide in water to 0.5 litre. Strong alkali: goggles and gloves.
Materiales para este paso:
Hidróxido de sodio — calidad de laboratorio180 gHerramientas necesarias:
Vaso de precipitados de borosilicato
Placa calefactora
Gafas de protección química
Guantes de goma3
3
Wash, dry and pre-heat at 700 °C
Wash, dry and pre-heat at 700 °C
Wash out the deposit, dry it, and pre-heat it at 700 °C so it moulds better.
Herramientas necesarias:
Papel de filtro
Agua destilada
Horno de secado
Horno tubular
Crisol con tapa (porcelana)
Guantes resistentes al calor4
4
Mould a ring at 4 tons per cm²
Mould a ring at 4 tons per cm²
Mould the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm section.
Herramientas necesarias:
Prensa hidráulica
Matriz de prensado anular
Mascarilla antipolvo5
5
Heat 3 hours at 900 °C, cool to 600 °C, hold 30 hours
Heat 3 hours at 900 °C, cool to 600 °C, hold 30 hours
Heat the ring for about 3 hours at 900 °C, cool it to 600 °C at 5 °C per minute, hold it there for 30 hours and let it cool to room temperature, all in a current of oxygen. Snoek's core: initial permeability 500.
Herramientas necesarias:
Horno tubular
Oxígeno
Bombona de gas a presión
Pirómetro
Tenazas para crisol
Guantes resistentes al calorMateriales
5- Marcador de posición
- 0.3 molMarcador de posición
- 1 molMarcador de posición
- Marcador de posición
- Marcador de posición
Herramientas requeridas
18- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Este plano hace
Blueprints relacionados
Estos blueprints comparten conocimiento — técnicas, materiales o principios
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.