Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)
Charlie

Creado por

Charlie

28. octubre 2026DE
6
0
0
0
0

Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)

A soft ferrite ring core of magnesium-zinc ferrite: magnesia, zinc oxide and iron oxide ground for a whole day, pressed into a ring and fired at 1400 °C in oxygen. Snoek's ring had an initial permeability of 670 and a Curie point near 100 °C. Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example II. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
Avanzado
2 days

Instrucciones

1

Weigh 25.5 : 25.5 : 49 mol %

Mix 25½ mol % pure magnesia, 25½ mol % pure zinc oxide and 49 mol % pure violet iron oxide. Ours, by weight: 9.4 g magnesium oxide, 18.99 g zinc oxide and 71.61 g iron oxide per 100 g. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.

Materiales para este paso:

Óxido de magnesioÓxido de magnesio9.4 g
Óxido de zinc en polvoÓxido de zinc en polvo18.99 g
Óxido de hierro violetaÓxido de hierro violeta71.61 g

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Mascarilla antipolvoMascarilla antipolvo
2

Grind for one day in an iron ball mill

Grind the mixture for one day in a mill with iron balls.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Mascarilla antipolvoMascarilla antipolvo
3

Press a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.

Herramientas necesarias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensado anularMatriz de prensado anular
Mascarilla antipolvoMascarilla antipolvo
4

Fire 1 hour at 1400 °C, cool slowly in oxygen

Heat the ring in oxygen for 1 hour at 1400 °C, then cool it slowly in oxygen. Snoek's ring had an initial permeability of 670 at room temperature and 2 kHz.

Herramientas necesarias:

Horno tubularHorno tubular
OxígenoOxígeno
Bombona de gas a presiónBombona de gas a presión
PirómetroPirómetro
Tenazas para crisolTenazas para crisol
Guantes resistentes al calorGuantes resistentes al calor

Materiales

3

Herramientas requeridas

11

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.