Glass Tube: Drawn by Two Glassmakers Walking Apart (Pellatt, 1849)
How glass tube was made by hand: a blown gather of glass is welded at one end to a second rod, and two workers walk away from each other while turning, stretching the hot glass into a tube up to 60 or 70 feet long. Because the whole bubble stretches evenly, the bore and the wall stay in the same proportion all along the tube.
Result: long glass tube of nearly even bore, cut into lengths when cold. Solid cane is made the same way without blowing.
Source: Apsley Pellatt, Curiosities of Glass Making (1849), pp. 106-108. Unknown: the glass batch and the gather's size. Picture: the book's figures.
Experto
Unknown
Instrucciones
1
1
Gather and blow the ball
Gather and blow the ball
Gather a solid ball of flint glass on the end of the blowing iron and blow it out a little, so it is hollow. When it has partly cooled, use it as a core for one or more further gatherings until there is enough glass. For flat-bore thermometer tube, flatten the first ball on the marver with an iron or wooden battledore before the later gatherings. Ours: lead crystal. Not given: the amount of glass.
Materiales para este paso:
Cristal de plomo1 flint glassHerramientas necesarias:
Horno de vidrio capaz de alcanzar 1100 grados Celsius
Caña de soplador de vidrio
Marver (placa de amasado del vidrio)2
2
Swing it long and fix the post
Swing it long and fix the post
Lengthen the ball by swinging it, and chill its far end by dipping it in cold water. A second worker makes a disc of hot glass on a rod, the 'post', and holds it upright near the ground. The chief worker climbs onto a chair and drops the hot ball onto the post, where it welds on.
Herramientas necesarias:
Agua
Puntel3
3
Walk apart and draw
Walk apart and draw
The chief worker steps down and the two walk away from each other, both turning their rods all the time. At first the hot glass sags between them in a curve; fan the parts that are thicker to cool them, so it stretches evenly. Draw it to the length wanted, up to 60 or 70 feet; as it cools it stops turning and pulls nearly straight. Except at the ends, it has nearly one bore, diameter and wall thickness. Ours: a wooden paddle for fanning (Pellatt: a boy's hat).
Herramientas necesarias:
Caña de soplador de vidrio
Puntel
Pala de madera4
4
Lay down and cut
Lay down and cut
Lay the tube across the wooden rungs of a ladder to cool. Cut it into lengths by touching it with a cold iron or nicking it with a steel file.
Herramientas necesarias:
Escalera de mano de madera
Lima para metalMateriales
1- 1 flint glassMarcador de posición
Herramientas requeridas
8- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Materiales de Blueprints conectados
Este plano hace
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.