Rasps: Teeth Raised One at a Time with a Pointed Punch
Forge

Creado por

Forge

11. octubre 2026NO
32
0
0
0
0

Rasps: Teeth Raised One at a Time with a Pointed Punch

A rasp is a coarse file whose teeth stand separately instead of in continuous rows. Each tooth is raised by driving a pointed punch into the face of the blank at uniform distances. Because the teeth stand apart, a rasp clogs less than a cut file on soft material such as wood or a horse's hoof. The blank is forged, annealed and ground like a file blank, and the finished rasp is hardened like a file: coated against scale, brought to a dull red heat and plunged into water, with the tang tempered so it will not snap. Machine-made rasps have uniformly stamped teeth, which line up row behind row and leave deeper marks; slightly uneven hand-cut teeth avoid this.
Avanzado
2 days (annealing overnight)

Instrucciones

1

Forge the blank

Forge the steel to a tapered bar, flat, round or half-round, with a narrow pointed tang at one end.

Materiales para este paso:

Tocho de acero al alto carbonoTocho de acero al alto carbono0.5 kg

Herramientas necesarias:

Fragua de herreroFragua de herrero
YunqueYunque
Martillo de forjaMartillo de forja
Tenazas de fraguaTenazas de fragua
2

Anneal and grind

Anneal the blank soft so the teeth can be raised, then grind the faces to a smooth, clear surface.

Herramientas necesarias:

Fragua de herreroFragua de herrero
Piedra de afilar de ruedaPiedra de afilar de rueda
3

Punch the teeth

Drive the pointed punch into the face with the hammer at uniform distances, raising one separate tooth at each blow. Turn the rasp over on a soft metal plate to work the other face without crushing the finished teeth.

Herramientas necesarias:

Punzón para escofinasPunzón para escofinas
Martillo de forjaMartillo de forja
YunqueYunque
Placa de peltrePlaca de peltre
4

Harden

Coat the toothed surface thickly with a salt composition against scaling, raise the rasp to a dull red heat in a clear coke fire and plunge it upright into water. If it bends, straighten it across a fulcrum before it is fully cold.

Materiales para este paso:

SalSal1 kg
Coque metalúrgicoCoque metalúrgico1 as required

Herramientas necesarias:

Fragua de herreroFragua de herrero
CuboCubo
Tenazas de fraguaTenazas de fragua
5

Temper the tang and clean

Temper the tang by dipping it in molten lead so it will not snap. Scour and wash off every trace of salt, then brush the rasp with oil.

Herramientas necesarias:

Baño de plomo fundidoBaño de plomo fundido
Tenazas de fraguaTenazas de fragua

Materiales

3

Herramientas requeridas

9

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...