Hard Porcelain Body: Kaolin, Felspar, Flint and Chalk, the Sèvres Paste
Hard porcelain is white kaolin made just fusible enough with ground felspar. Andrew Ure (1839) gives the Sèvres paste: 63–70 parts washed kaolin, 22–15 felspar, about 10 flint powder and 5 chalk, mixed as slips, stiffened on plaster and left to ripen damp for months before it is trodden and used.
The picture: centring porcelain paste on the wheel in the Grand Atelier of the Sèvres manufactory.
Avanzado
Days to mix, months to ripen
Instrucciones
1
1
Calcine and grind the felspar
Calcine and grind the felspar
Pick felspar free of dark mica and rust. Heat it red hot in the kiln and quench it so it crumbles, then crush and grind it very fine with water and sift.
Materiales para este paso:
Trozo de feldespato2 kg
Agua10 litrosHerramientas necesarias:
Horno cerámico
Cubo de temple
Mortero y mano de mortero
Moleta
Tamiz de malla fina
Guantes resistentes al calor
Mascarilla antipolvo2
2
Flint powder
Flint powder
Calcine and quench flint the same way and grind it to a fine powder with water.
Materiales para este paso:
Nódulo de sílex1 kgHerramientas necesarias:
Horno cerámico
Cubo de temple
Moleta
Tamiz de malla fina
Mascarilla antipolvo3
3
Weigh and mix the slips
Weigh and mix the slips
Weigh the dry kaolin, felspar, flint and chalk in Ure's proportions, stir each into water and mix them into one smooth slip; pass it through a fine sieve.
Materiales para este paso:
Caolín en polvo6.65 kg
Carbonato de calcio (blanco de España)0.5 kg
Agua15 litrosHerramientas necesarias:
Balanza de platillos
Cuba
Tamiz de malla fina4
4
Stiffen on plaster, ripen
Stiffen on plaster, ripen
Pour the slip onto plaster bats to draw the water out without heat. When it is a soft paste, store it covered and damp for months to ripen.
Herramientas necesarias:
Base de escayola para alfarería5
5
Tread and ball it
Tread and ball it
Before use, work the paste hard on the wedging table (Sèvres trod it barefoot) until even, and keep it in damp balls.
Herramientas necesarias:
Mesa de amasado de arcilla6
6
Ure's Sèvres paste, scaled
Ure's Sèvres paste, scaled
Cargando el cuaderno de Jupyter…
7
7
Limits
Limits
The recipe and handling are Ure's; calcining the flint and the batch size are ours. Grinding flint and felspar makes fine silica dust that harms the lungs over time: grind wet and wear a mask.
Materiales
5- Marcador de posición
- 25 litrosMarcador de posición
- 1 kgMarcador de posición
- 6.65 kgMarcador de posición
- Marcador de posición
Herramientas requeridas
11- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Este plano hace
Blueprints relacionados
Estos blueprints comparten conocimiento — técnicas, materiales o principios
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.