Oriented Barium Ferrite Disc Magnet: Weak 2000 Oersted Field, Then Pressed (Gorter, Philips 1956, Ex. 2)
Charlie

Creado por

Charlie

28. octubre 2026DE
11
0
0
0
0

Oriented Barium Ferrite Disc Magnet: Weak 2000 Oersted Field, Then Pressed (Gorter, Philips 1956, Ex. 2)

A ceramic magnet from pre-fired barium ferrite powder suspended in polyvinyl acetate in acetone, oriented in a weak 2000 oersted field, then pressed into a block, heated to 500 °C in a field and sintered at 1300 °C. In the principal direction it held 2,550 gauss with a coercive force of 1,750 oersted and a (BH)max of 1.13 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 2. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
3 days

Instrucciones

1

Weigh barium carbonate and iron oxide

Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiales para este paso:

Carbonato de bario (witherita)Carbonato de bario (witherita)450 g
Óxido férricoÓxido férrico2000 g

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Guantes de gomaGuantes de goma
Respirador P100Respirador P100
2

Mill 20 hours under alcohol, dry

Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
3

Pre-fire: through a 1100 °C zone in 10 minutes

Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.

Herramientas necesarias:

Horno tubularHorno tubular
Crisol con tapa (porcelana)Crisol con tapa (porcelana)
Guantes resistentes al calorGuantes resistentes al calor
4

Grind 12 hours with alcohol, dry

Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 4 cc of solution per 3 g of powder. The binder burns off later.

Herramientas necesarias:

Poliacetato de viniloPoliacetato de vinilo
AcetonaAcetona
Balanza de platillosBalanza de platillos
6

Orient in a 2000 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 2000 oersted. Switch the field off and remove the binder solution.

Herramientas necesarias:

Matriz de prensado de discosMatriz de prensado de discos
ElectroimánElectroimán
Prensa hidráulicaPrensa hidráulica
7

Compress into a block

Compress the powder into a block. The pressure is not given.

Herramientas necesarias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
8

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Herramientas necesarias:

Horno tubularHorno tubular
ElectroimánElectroimán
Guantes resistentes al calorGuantes resistentes al calor
9

Sinter: through a 1300 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1300 °C with a 10 cm hot zone: about 5 minutes in the heat.

Herramientas necesarias:

Horno tubularHorno tubular
Guantes resistentes al calorGuantes resistentes al calor
10

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

Herramientas necesarias:

ElectroimánElectroimán
BrújulaBrújula

Materiales

2

Herramientas requeridas

15

Blueprints relacionados

Estos blueprints comparten conocimiento — técnicas, materiales o principios

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...