Oriented Barium Ferrite Disc Magnet: Binder Dried in a 2400 Oersted Field (Gorter, Philips 1956, Ex. 3)
A ceramic magnet from pre-fired barium ferrite in polyvinyl acetate and acetone, dried in a 2400 oersted field, then pressed, heated and sintered as in Example 2. In the principal direction it held 2,720 gauss with a coercive force of 1,620 oersted and a (BH)max of 1.2 × 10⁶; at right angles 1,610 gauss.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 3. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
3 days
Instrucciones
1
1
Weigh barium carbonate and iron oxide
Weigh barium carbonate and iron oxide
Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Materiales para este paso:
Carbonato de bario (witherita)450 g
Óxido férrico2000 gHerramientas necesarias:
Balanza de platillos
Guantes de goma
Respirador P1002
2
Mill 20 hours under alcohol, dry
Mill 20 hours under alcohol, dry
Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.
Herramientas necesarias:
Molino de bolas de hierro
Etanol de laboratorio, 95 %
Horno de secado3
3
Pre-fire: through a 1100 °C zone in 10 minutes
Pre-fire: through a 1100 °C zone in 10 minutes
Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.
Herramientas necesarias:
Horno tubular
Crisol con tapa (porcelana)
Guantes resistentes al calor4
4
Grind 12 hours with alcohol, dry
Grind 12 hours with alcohol, dry
Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.
Herramientas necesarias:
Molino de bolas de hierro
Etanol de laboratorio, 95 %
Horno de secado5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 2 cc of solution per gram of powder. The binder burns off later.
Herramientas necesarias:
Poliacetato de vinilo
Acetona
Balanza de platillos6
6
Orient in a 2400 oersted field
Orient in a 2400 oersted field
Put the suspension in a moulding die between the poles of a magnet and apply a first field of 2400 oersted. Remove the binder solution while the field is on.
Herramientas necesarias:
Matriz de prensado de discos
Electroimán
Prensa hidráulica7
7
Compress into a block
Compress into a block
Compress the powder into a block as in Example 2. The pressure is not given.
Herramientas necesarias:
Prensa hidráulica
Matriz de prensado de discos8
8
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Herramientas necesarias:
Horno tubular
Electroimán
Guantes resistentes al calor9
9
Sinter: through a 1300 °C zone in 5 minutes
Sinter: through a 1300 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1300 °C with a 10 cm hot zone: about 5 minutes in the heat.
Herramientas necesarias:
Horno tubular
Guantes resistentes al calor10
10
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Herramientas necesarias:
Electroimán
BrújulaMateriales
2- Marcador de posición
- 2000 gMarcador de posición
Herramientas requeridas
15- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Este plano hace
Blueprints relacionados
Estos blueprints comparten conocimiento — técnicas, materiales o principios
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.