Oriented Barium Ferrite Disc Magnet: Heated to 500 °C Without a Field (Gorter, Philips 1956, Ex. 6)
A ceramic magnet oriented in the die as in Example 4, but heated to 500 °C with no second field before sintering at 1280 °C. In the principal direction it held 3,025 gauss with a coercive force of 1,550 oersted and a (BH)max of 1.58 × 10⁶.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 6. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
3 days
Instrucciones
1
1
Weigh barium carbonate and iron oxide
Weigh barium carbonate and iron oxide
Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Materiales para este paso:
Carbonato de bario (witherita)450 g
Óxido férrico2000 gHerramientas necesarias:
Balanza de platillos
Guantes de goma
Respirador P1002
2
Mill 20 hours under alcohol, dry
Mill 20 hours under alcohol, dry
Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.
Herramientas necesarias:
Molino de bolas de hierro
Etanol de laboratorio, 95 %
Horno de secado3
3
Pre-fire: through a 1100 °C zone in 10 minutes
Pre-fire: through a 1100 °C zone in 10 minutes
Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.
Herramientas necesarias:
Horno tubular
Crisol con tapa (porcelana)
Guantes resistentes al calor4
4
Grind 12 hours with alcohol, dry
Grind 12 hours with alcohol, dry
Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.
Herramientas necesarias:
Molino de bolas de hierro
Etanol de laboratorio, 95 %
Horno de secado5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.
Herramientas necesarias:
Poliacetato de vinilo
Acetona
Balanza de platillos6
6
Orient in a 10000 oersted field
Orient in a 10000 oersted field
Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on (as in Example 4).
Herramientas necesarias:
Matriz de prensado de discos
Electroimán
Prensa hidráulica7
7
Heat to 500 °C without a field
Heat to 500 °C without a field
Heat the blocks to 500 °C with no magnetic field.
Herramientas necesarias:
Horno tubular
Guantes resistentes al calor8
8
Sinter: through a 1280 °C zone in 5 minutes
Sinter: through a 1280 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.
Herramientas necesarias:
Horno tubular
Guantes resistentes al calor9
9
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Herramientas necesarias:
Electroimán
BrújulaMateriales
2- Marcador de posición
- 2000 gMarcador de posición
Herramientas requeridas
15- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Este plano hace
Blueprints relacionados
Estos blueprints comparten conocimiento — técnicas, materiales o principios
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.