A strontium ferrite magnet oriented in a magnetic field: strontium carbonate and iron oxide milled, pre-fired 2 hours at 1000 °C, ground fine in an agate mill, then oriented, heated and sintered as in Example 4. In the principal direction it held 2,640 gauss with a coercive force of 2,825 oersted and a (BH)max of 1.63 × 10⁶.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 8. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
3 days
Instrucciones
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g strontium carbonate and 179 g ferric oxide.
Materiales para este paso:
Carbonato de estroncio29.5 g
Óxido férrico179 gHerramientas necesarias:
Balanza de platillos
Respirador P1002
2
Mill 15 hours with alcohol, dry
Mill 15 hours with alcohol, dry
Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.
Herramientas necesarias:
Molino de bolas de hierro
Etanol de laboratorio, 95 %
Horno de secado3
3
Pre-fire 2 hours at 1000 °C in air
Pre-fire 2 hours at 1000 °C in air
Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.
Herramientas necesarias:
Horno mufla
Crisol con tapa (porcelana)
Tenazas para crisol
Guantes resistentes al calor4
4
Grind 4 hours in an agate centrifugal mill
Grind 4 hours in an agate centrifugal mill
Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder.
Herramientas necesarias:
Molino centrífugo de ágata
Etanol de laboratorio, 95 %
Horno de secado5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.
Herramientas necesarias:
Poliacetato de vinilo
Acetona
Balanza de platillos6
6
Orient in a 10000 oersted field
Orient in a 10000 oersted field
Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on.
Herramientas necesarias:
Matriz de prensado de discos
Electroimán
Prensa hidráulica7
7
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Herramientas necesarias:
Horno tubular
Electroimán
Guantes resistentes al calor8
8
Sinter: through a 1280 °C zone in 5 minutes
Sinter: through a 1280 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.
Herramientas necesarias:
Horno tubular
Guantes resistentes al calor9
9
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Herramientas necesarias:
Electroimán
BrújulaMateriales
2- 29.5 gMarcador de posición
- 179 gMarcador de posición
Herramientas requeridas
17- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Este plano hace
Blueprints relacionados
Estos blueprints comparten conocimiento — técnicas, materiales o principios
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.