A plaster bat is a round slab of plaster that potters use to hold work while making or drying it, and to stiffen wet clay. Binns makes his first one in a frying pan. Variable: plaster per quart of water. 2 3/4 lb is his standard; less gives a softer bat, more a harder one. Source: Charles F. Binns, The Potter's Craft (1910), pp. 43-47. Picture: drawn by Youblob from the text.
Principiante
Unknown

Instrucciones

1

Make the size

Put a quart of water in a kettle with a piece of soft soap the size of an egg. Simmer about an hour, until the soap has dissolved, and let it cool. Cold, it should be like maple syrup. The size keeps plaster from sticking to a surface.

Herramientas necesarias:

AguaAgua
Material desconocidoMaterial desconocido
Cazo altoCazo alto
2

Size the frying pan

Brush size onto the inside of the pan, wipe it off with a sponge, then wash with a second sponge and clean water. On metal one coat often does; repeat until the surface rejects water like grease. On the last coat don't wash: polish with the size sponge. Set the pan on a level table.

Herramientas necesarias:

Sartén de acero al carbonoSartén de acero al carbono
Pinceles finosPinceles finos
EsponjaEsponja
3

Mix the plaster

Take as much water as fills the pan about 1 in deep; Binns supposes a quart. Weigh 2 3/4 lb of dry potters' plaster for each quart and let it trickle through your fingers into the water in a jug. After about two minutes, when it has soaked up all the water it will take, stir with your hand to a smooth cream, breaking all lumps and removing air bubbles.

Materiales para este paso:

EscayolaEscayola2.75 libras
AguaAgua1 quart

Herramientas necesarias:

Jarra medidoraJarra medidora
BalanzaBalanza
4

Pour at the right moment

Keep stirring gently until the mix thickens and leaves a white coating on your hand that won't shake off. Then pour it into the pan and shake gently to level it. Poured right, it sets smooth and mat, like sugar icing. Poured too late, it is stiff and hard to level; too soon, it curdles with water on top. Wash the jug at once in a tub, never down a sink: plaster chokes the drain.

Herramientas necesarias:

Sartén de acero al carbonoSartén de acero al carbono
TinaTina
5

Turn out and scrape the bat

After about ten minutes the bat grows warm: setting is complete. Hold the pan upside down by the handle and rap its edge smartly on a brick or stone. The disc falls out. Scrape its edge and set it aside. Binns suggests making half a dozen for practice.

Herramientas necesarias:

Sartén de acero al carbonoSartén de acero al carbono
Rasqueta de aceroRasqueta de acero

Materiales

2
  • 2.75 libras
    Marcador de posición
  • 1 quart
    Marcador de posición

Herramientas requeridas

10

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...