Precipitated Silica: Hot Water Glass Carbonated, Then Acidified to pH 6.75 (Allen 1957)

Bubble carbon dioxide through hot dilute water glass and the silica comes down as an extremely fine white powder rather than a gel. Edward Allen of Columbia-Southern made it this way as a white reinforcing filler for rubber; this follows his Example XI, which gave a powder of 148 m² per gram. Source: E. M. Allen (Columbia-Southern), US 2,805,955 (1957), Example XI. The percentages are our arithmetic; the filter, mill and indicator are ours. Picture drawn by Youblob.
Intermedio
2 days

Instrucciones

1

Dilute the water glass

Take 12,850 g of sodium silicate solution holding 976 g Na2O and 3115 g SiO2 (7.6 % and 24.2 %, a silica to soda ratio of 3.19 by weight; our arithmetic). Dilute it with water to 48 litres in a stirred kettle with a heating coil and thermometer, and heat to 95 °C.

Materiales para este paso:

Vidrio soluble (solución de silicato de sodio)Vidrio soluble (solución de silicato de sodio)12850 g
AguaAgua1 as required

Herramientas necesarias:

Reactor a presiónReactor a presión
AgitadorAgitador
TermómetroTermómetro
Balanza de platillosBalanza de platillos
2

Carbonate for an hour

Bubble in pure carbon dioxide fast enough to add the theoretical amount in about 30 minutes, and keep going at that rate for about 1 hour. The slurry ends at pH 9.85.

Herramientas necesarias:

Dióxido de carbono gaseosoDióxido de carbono gaseoso
Reactor a presiónReactor a presión
AgitadorAgitador
TermómetroTermómetro
Papel indicador de pHPapel indicador de pH
3

Filter and wash

Filter the slurry and wash the cake twice with hot water.

Materiales para este paso:

AguaAgua1 as required

Herramientas necesarias:

Embudo Buchner (de porcelana)Embudo Buchner (de porcelana)
Papel de filtroPapel de filtro
4

Acidify to pH 6.75

Stir the cake back into water and bring it to pH 6.75 with 400 ml of 3.5 N hydrochloric acid.

Materiales para este paso:

AguaAgua1 as required

Herramientas necesarias:

Ácido clorhídricoÁcido clorhídrico
Recipiente de vidrioRecipiente de vidrio
AgitadorAgitador
Papel indicador de pHPapel indicador de pH
5

Wash out the chloride

Filter again and wash the cake with hot water until it is nearly free of chloride.

Materiales para este paso:

AguaAgua1 as required

Herramientas necesarias:

Embudo Buchner (de porcelana)Embudo Buchner (de porcelana)
Papel de filtroPapel de filtro
6

Dry at 105 °C and grind

Dry it at 105 °C in a fan oven and grind it to a fine powder. Allen's had a pH of 8.2, 0.61 % sodium and a surface area of 148 m² per gram.

Herramientas necesarias:

Horno de secadoHorno de secado
Mortero y mano de morteroMortero y mano de mortero
Tarros de vidrio con tapaTarros de vidrio con tapa

Materiales

2

Herramientas requeridas

13

Blueprints relacionados

Estos blueprints comparten conocimiento — técnicas, materiales o principios

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...