Precipitated Silver: Silver Chloride Reduced by Zinc in Acidulated Water (Thorpe 1913)

Fine silver powder without melting anything. Hydrochloric acid throws silver out of solution as white silver chloride. Zinc in slightly acid water then takes the chlorine away and leaves the silver as a grey powder. Source: Thorpe, Dictionary of Applied Chemistry, vol. 4 (1913), Silver. Thorpe gives no amounts, times or end-point. Ours: a silver nitrate solution, zinc sheet strips, hydrochloric acid of the two acids he names, and the washing and drying. Picture drawn by Youblob.
Principiante
1 day

Instrucciones

1

Dissolve silver nitrate in water

Ours: dissolve silver nitrate in distilled water as the silver solution. Silver nitrate stains and burns skin: gloves and goggles.

Materiales para este paso:

Nitrato de plataNitrato de plata1 as required
Agua destiladaAgua destilada1 as required

Herramientas necesarias:

Vaso de precipitados de borosilicatoVaso de precipitados de borosilicato
Varilla de vidrio borosilicatoVarilla de vidrio borosilicato
Guantes de nitriloGuantes de nitrilo
Gafas de protección químicaGafas de protección química
2

Throw down silver chloride with hydrochloric acid

Add hydrochloric acid to the solution. White silver chloride falls. Ours: add it while it still makes a precipitate, let it settle and pour off the liquid.

Materiales para este paso:

Ácido clorhídricoÁcido clorhídrico1 as required

Herramientas necesarias:

Vaso de precipitados de borosilicatoVaso de precipitados de borosilicato
Varilla de vidrio borosilicatoVarilla de vidrio borosilicato
Guantes de nitriloGuantes de nitrilo
Gafas de protección químicaGafas de protección química
3

Reduce the chloride with zinc in acid water

Cover the chloride with water made slightly acid with hydrochloric acid (Thorpe: hydrochloric or sulphuric) and put zinc in it. The zinc reduces the chloride to silver. Ours: strips of zinc sheet, left in until no white chloride is left. Time not given.

Materiales para este paso:

Chapa de cincChapa de cinc1 as required
Ácido clorhídricoÁcido clorhídrico1 as required
Agua destiladaAgua destilada1 as required

Herramientas necesarias:

Vaso de precipitados de borosilicatoVaso de precipitados de borosilicato
Varilla de vidrio borosilicatoVarilla de vidrio borosilicato
Guantes de nitriloGuantes de nitrilo
Gafas de protección químicaGafas de protección química
4

Take out the zinc, wash and dry the silver

Ours: lift out what is left of the zinc, wash the grey silver powder with water until the washings are no longer acid, filter, and dry it. Keep it in a closed jar.

Herramientas necesarias:

Agua destiladaAgua destilada
Papel de filtroPapel de filtro
Horno de secadoHorno de secado
Tarro de vidrioTarro de vidrio

Materiales

4

Herramientas requeridas

8

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...