Silicone Rubber Compound: Dimethyl Silicone Oil Gelled with Ferric Oxide, Agens 1948
Mary

Creado por

Mary

17. octubre 2026FI
6
0
0
0
0

Silicone Rubber Compound: Dimethyl Silicone Oil Gelled with Ferric Oxide, Agens 1948

Dimethyl silicone oil mixed with three-quarters its weight of red ferric oxide and a little aluminium chloride, heated to 130 °C, thins and then sets to a solid mass; milled on warm rubber rolls it becomes a silicone rubber compound ready to mould or extrude (Agens, General Electric, US 2,448,756, 1948). Cured, it stretches over 100 % and stays flexible at −60 °C. The picture: our drawing of the beaker, the mill and the sheet.
Avanzado
A day

Instrucciones

1

Weigh the mix

To 400 g silicone oil add 300 g ferric oxide (75 % of the oil) and 5 g anhydrous aluminium chloride (1.25 %). Stir it smooth. Keep the chloride dry; it fumes in damp air.

Materiales para este paso:

Aceite de dimetilsiliconaAceite de dimetilsilicona400 g
Polvo de rojo de pulir finoPolvo de rojo de pulir fino300 g

Herramientas necesarias:

Cloruro de aluminio (anhidro)Cloruro de aluminio (anhidro)
Vaso de precipitados de borosilicatoVaso de precipitados de borosilicato
AgitadorAgitador
Báscula digital de cocinaBáscula digital de cocina
Guantes de gomaGuantes de goma
2

Heat to 130 °C

Heat the mix to 130 °C. It first gets thinner, then thickens fast until the whole mass is solid.

Herramientas necesarias:

Placa calefactoraPlaca calefactora
TermómetroTermómetro
Vaso de precipitados de borosilicatoVaso de precipitados de borosilicato
3

Mill and sheet

Work the mass on rubber rolls at 125 °C for about half an hour and take it off as a sheet. This is the compound.

Herramientas necesarias:

Molino de dos rodillos para cauchoMolino de dos rodillos para caucho
TermómetroTermómetro
4

Test a piece

Agens's test: press a sheet about 1.3 mm thick between platens at 150 °C for ten minutes, then 15 minutes in an oven at 200 °C. It should stretch over twice its length.

Herramientas necesarias:

Prensa calefactada de moldeo por compresiónPrensa calefactada de moldeo por compresión
Horno de recocidoHorno de recocido
5

The mix

Cargando el cuaderno de Jupyter…

Materiales

2

Herramientas requeridas

10

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...