Silver Oxide: Silver Nitrate Precipitated with Solution of Potassa (USP 1870)

Silver oxide is a heavy, dark brown powder, and heating it to about 250 °C leaves pure silver. Potash added to a silver nitrate solution throws it down, and washing leaves potassium nitrate behind in the water. Source: US Pharmacopoeia 1870, as quoted in the US Dispensatory (1907), Argenti Oxidum. Not given here: the strength of the solution of potassa; ours: potassium hydroxide in distilled water. Silver nitrate stains and burns skin: gloves and goggles. Picture drawn by Youblob.
Principiante
1 day

Instrucciones

1

Dissolve 4 troy oz silver nitrate in half a pint of water

Dissolve 4 troy ounces of silver nitrate in half a pint of distilled water. Silver nitrate stains and burns skin: gloves and goggles.

Materiales para este paso:

Nitrato de plataNitrato de plata4 troy oz
Agua destiladaAgua destilada0.5 pint

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Vaso de precipitados de borosilicatoVaso de precipitados de borosilicato
Varilla de vidrio borosilicatoVarilla de vidrio borosilicato
Guantes de nitriloGuantes de nitrilo
Gafas de protección químicaGafas de protección química
2

Add solution of potassa while it still precipitates

Add solution of potassa, about a pint and a half or as much as needed, for as long as it still throws down a precipitate. Ours: potassium hydroxide dissolved in distilled water; the USP strength is not given here. Potash free of carbon dioxide keeps out silver carbonate.

Materiales para este paso:

Hidróxido de potasioHidróxido de potasio1 as required
Agua destiladaAgua destilada1.5 pint

Herramientas necesarias:

Vaso de precipitados de borosilicatoVaso de precipitados de borosilicato
Varilla de vidrio borosilicatoVarilla de vidrio borosilicato
Guantes de nitriloGuantes de nitrilo
Gafas de protección químicaGafas de protección química
3

Wash, dry and store in the dark

Wash the precipitate again and again with water until the washings are almost tasteless. Dry it and keep it in a well-stoppered bottle away from light. Ours: filter paper, and a low oven, well below the 250 °C at which it breaks down to silver.

Herramientas necesarias:

Papel de filtroPapel de filtro
Agua destiladaAgua destilada
Horno de secadoHorno de secado
Tarros de vidrio oscuro con cierre herméticoTarros de vidrio oscuro con cierre hermético

Materiales

3

Herramientas requeridas

9

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...