Stone Flat Chisel: the Marble Lettering Tool, Drawn Very Thin (Holford, 1907)
Forge

Creado por

Forge

5. noviembre 2026NO
18
0
0
0
0

Stone Flat Chisel: the Marble Lettering Tool, Drawn Very Thin (Holford, 1907)

A flat chisel for cutting letters in marble. Frederick Holford's 20th Century Toolsmith (1907) makes marble tools like granite tools, from 7/8-inch octagon steel, but tempers them a little harder, to a very light straw. The lettering tool is drawn out very thin (his Fig. 69); because of that thinness it must be heated with great care, and the last few blows when dressing it are struck on the flat side only, at a very low heat. He gives no edge width, length or carbon content; those are unknown here. Source: F. J. Holford, The 20th Century Toolsmith and Steelworker (1907), p. 130, pp. 122-123 and p. 21 (the hardening bath). Picture: his Fig. 69.
Intermedio
An hour

Instrucciones

1

Read Holford

"Lettering tools are drawn out very thin, as Fig. 69, but owing to the thinness be very careful when heating, and make sure when dressing to always strike the last few blows on the flat side only, when at a very low heat."
2

Draw out the edge

Forge 7/8-inch octagon steel down to a straight edge, drawn out very thin (Fig. 69). Heat with great care because of the thinness. Strike the last few blows on the flat side only, at a very low heat. Straighten the edge with a very coarse file after hammering. Edge width and length are not given (unknown).

Materiales para este paso:

Barra octogonal de acero para herramientasBarra octogonal de acero para herramientas1 bar

Herramientas necesarias:

FraguaFragua
YunqueYunque
Martillo de herreroMartillo de herrero
Tenazas de herreroTenazas de herrero
Lima para metalLima para metal
Dimensiones desconocidasDimensiones desconocidas
3

Harden and temper

Heat no farther back than 1/2 inch, taking care not to overheat the thin edge. Dip at least an inch deep into the hardening bath (p. 21: clean water, best a brine with as much salt as it will dissolve, large and cold) so the temper runs back slowly, and stop it at a very light straw, the marble temper.

Herramientas necesarias:

FraguaFragua
Tenazas de herreroTenazas de herrero
Salmuera saturadaSalmuera saturada
Guantes resistentes al calorGuantes resistentes al calor
4

History and honest limits

Holford sets lettering tools apart from the tooth and plain chisels used to dress marble, which "are not drawn out so thin"; the teeth of tooth chisels are filed in after hammering (his Fig. 70). Edge width, length and the carbon of the steel are not given; an octagonal tool steel bar stands for the 7/8-inch octagon steel.

Materiales

1

Herramientas requeridas

8

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...