Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)
Charlie

Creado por

Charlie

28. octubre 2026DE
4
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)

A strontium ferrite with a fifth of the strontium replaced by calcium: 0.08 mol strontium carbonate and 0.02 mol calcium carbonate to 0.6 mol iron oxide, ground, dried, formed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 2,320 gauss with a coercive force of 1,395 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 23. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
2 days

Instrucciones

1

Weigh the carbonates and iron oxide

Weigh 11.81 g strontium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol), 95.55 g ferric oxide (0.6 mol).

Materiales para este paso:

Carbonato de estroncioCarbonato de estroncio11.81 g
Carbonato de calcio (blanco de España)Carbonato de calcio (blanco de España)2.002 g
Óxido férricoÓxido férrico95.55 g

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Respirador P100Respirador P100
2

Mill with alcohol 4 hours, dry

As in Examples 18 to 21: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
3

Press at 1.5 t/cm²

Example 23 does not say whether the 1000 °C presinter of Examples 18 to 21 is used. Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Herramientas necesarias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Herramientas necesarias:

Horno tubularHorno tubular
Guantes resistentes al calorGuantes resistentes al calor
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Herramientas necesarias:

ElectroimánElectroimán
BrújulaBrújula

Materiales

3

Herramientas requeridas

11

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...