Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)
A strontium ferrite magnet made exactly like Went's barium ferrite of Example 34, with strontium carbonate in place of barium carbonate: 29.5 g of it to 191.7 g iron oxide, milled, fired, milled again, pressed and sintered for 4 hours. This iteration sinters at 1200 °C, where his rod held 1,340 gauss with a coercive force of 3,900 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 34. They pressed rods; the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
2 days
Instrucciones
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g of strontium carbonate and 191.7 g of ferric oxide, Fe2O3. The patent makes this second mixture "in exactly the same manner" as the barium one.
Materiales para este paso:
Carbonato de estroncio29.5 g
Óxido férrico191.7 gHerramientas necesarias:
Balanza de platillos
Guantes de goma
Respirador P1002
2
Mill with ethanol for 4 hours
Mill with ethanol for 4 hours
Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.
Herramientas necesarias:
Molino de bolas de hierro
Etanol de laboratorio, 95 %
Horno de secado3
3
Presinter at 1000 °C for 4 hours
Presinter at 1000 °C for 4 hours
Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.
Herramientas necesarias:
Horno mufla
Crisol con tapa (porcelana)
Tenazas para crisol
Guantes resistentes al calor4
4
Mill again for 4 hours
Mill again for 4 hours
Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.
Herramientas necesarias:
Molino de bolas de hierro
Etanol de laboratorio, 95 %
Horno de secado
Respirador P1005
5
Press discs at 1.5 tons per cm²
Press discs at 1.5 tons per cm²
Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).
Herramientas necesarias:
Prensa hidráulica
Matriz de prensado de discos6
6
Sinter 4 hours at 1200 °C
Sinter 4 hours at 1200 °C
Sinter the discs for 4 hours at 1200 °C in oxygen or in air. The patent's strontium rod at 1200 °C: 1,340 gauss and 3,900 oersted.
Herramientas necesarias:
Horno mufla
Tenazas para crisol
Guantes resistentes al calor7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Herramientas necesarias:
Electroimán
BrújulaMateriales
2- 29.5 gMarcador de posición
- 191.7 gMarcador de posición
Herramientas requeridas
14- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
- Marcador de posición
Este plano hace
Blueprints relacionados
Estos blueprints comparten conocimiento — técnicas, materiales o principios

Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
por Charlie
Industrial
11
0
0
0
0
0

Strontium Carbonate: Powdered Celestine Boiled with Soda Solution (Thorpe 1912)
por Charlie
Industrial
14
0
0
0
0
0

Peligroso
Ferrite Toroid Core: Nickel-Zinc Ferrite Sintered at 1300 °C in Oxygen (Snoek)
por Charlie
Industrial
17
0
0
0
0
0

Ferric Oxide: Hydroxide Precipitated from Ferric Chloride with Ammonia, Then Heated
por Charlie
Inorgánico
12
0
0
0
0
0
CC0 Dominio público
Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.
Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.