Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1300 °C (Went, Philips 1956, Ex. 34)

A strontium ferrite magnet made exactly like Went's barium ferrite of Example 34, with strontium carbonate in place of barium carbonate: 29.5 g of it to 191.7 g iron oxide, milled, fired, milled again, pressed and sintered for 4 hours. This iteration sinters at 1300 °C, where his rod held 1,850 gauss with a coercive force of 2,130 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 34. They pressed rods; the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzado
2 days

Instrucciones

1

Weigh strontium carbonate and iron oxide

Weigh 29.5 g of strontium carbonate and 191.7 g of ferric oxide, Fe2O3. The patent makes this second mixture "in exactly the same manner" as the barium one.

Materiales para este paso:

Carbonato de estroncioCarbonato de estroncio29.5 g
Óxido férricoÓxido férrico191.7 g

Herramientas necesarias:

Balanza de platillosBalanza de platillos
Guantes de gomaGuantes de goma
Respirador P100Respirador P100
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

Herramientas necesarias:

Horno muflaHorno mufla
Crisol con tapa (porcelana)Crisol con tapa (porcelana)
Tenazas para crisolTenazas para crisol
Guantes resistentes al calorGuantes resistentes al calor
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

Herramientas necesarias:

Molino de bolas de hierroMolino de bolas de hierro
Etanol de laboratorio, 95 %Etanol de laboratorio, 95 %
Horno de secadoHorno de secado
Respirador P100Respirador P100
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

Herramientas necesarias:

Prensa hidráulicaPrensa hidráulica
Matriz de prensado de discosMatriz de prensado de discos
6

Sinter 4 hours at 1300 °C

Sinter the discs for 4 hours at 1300 °C in oxygen or in air. The patent's strontium rod at 1300 °C: 1,850 gauss and 2,130 oersted.

Herramientas necesarias:

Horno muflaHorno mufla
Tenazas para crisolTenazas para crisol
Guantes resistentes al calorGuantes resistentes al calor
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Herramientas necesarias:

ElectroimánElectroimán
BrújulaBrújula

Materiales

2

Herramientas requeridas

14

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...