Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)
Charlie

Creado por

Charlie

1. noviembre 2026DE
7
0
0
0
0

Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)

Ytterbium boils far more easily than lanthanum. Heated with lanthanum in a vacuum, ytterbium oxide gives up its oxygen to the lanthanum, and the freed ytterbium leaves as vapour and condenses in a cooler zone, while lanthanum oxide stays behind. Result: ytterbium metal ingots; 20 kg of distillate in the patent's run, low in sodium, potassium and lithium. Source: Y. Shindo and K. Yagi, US patent application 2010/0260640 (2010), Example 1. Not given: how much lanthanum, the vacuum, the time, crucible and condenser materials. Picture drawn by Youblob.
Avanzado
1 day

Instrucciones

1

Mix the oxide with lanthanum

Mix ytterbium oxide with lanthanum metal as the reducing agent. Not given: the proportions.

Materiales para este paso:

Óxido de iterbioÓxido de iterbio1 as required

Herramientas necesarias:

LantanoLantano
Crisol de tántaloCrisol de tántalo
2

Reduce in vacuum at 1020 °C

Heat the charge in a vacuum to 1020 °C: Yb2O3 + 2 La -> 2 Yb (vapour) + La2O3. Ours: a vacuum induction furnace; the vacuum level and time are not given.

Herramientas necesarias:

Horno de inducciónHorno de inducción
Bomba de vacíoBomba de vacío
Crisol de tántaloCrisol de tántalo
3

Condense the ytterbium at 200-600 °C

Catch the ytterbium vapour on a condenser held at 200-600 °C. Most of it settles in the 300-500 °C part; the 200-300 °C part carries the least sodium and lithium. Ours: a tantalum condenser plate.

Herramientas necesarias:

Placa condensadora de tántaloPlaca condensadora de tántalo
4

Melt into ingots under argon

Take the distillate off the condenser, melt it in a crucible at 950 °C under a slight pressure of argon, and let it solidify into an ingot.

Herramientas necesarias:

Crisol de tántaloCrisol de tántalo
Horno de inducciónHorno de inducción
ArgónArgón

Materiales

1

Herramientas requeridas

6

Este plano hace

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...