Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass

A thick acrylic block cannot be cast flawless in one pour. Tattersall (ICI, US 2,071,907, 1937) built it up in layers: pour 1/2 inch of syrup on a level glass plate, let it set for a day at room temperature, pour the next 1/2 inch on top, cover with a second glass plate, wait another day, then heat the sandwich at 80 °C. Each 1/2 inch layer shrinks to about 1/3 inch. The glass gives both faces a finished polish with no grinding. The picture: our diagram.
Intermédiaire
3 days

Consignes

1

Level the bottom plate

Set a glass plate on a ledge in a wooden frame, on a body of plaster of Paris, and level it carefully. The example sheet was 10 by 18 inches.

Outils nécessaires :

VitreVitre
Cadre en boisCadre en bois
Plâtre de ParisPlâtre de Paris
Niveau à bulle de 1,5 mNiveau à bulle de 1,5 m
2

Pour the first 1/2 inch

Pour room-temperature syrup 1/2 inch deep (about 1.5 litres for 10 by 18 inches; our figure). Cover against dust, but do not put the top plate on yet. Leave 24 hours at about 20 °C.

Matériaux pour cette étape :

Sirop de méthacrylate de méthyleSirop de méthacrylate de méthyle3 l

Outils nécessaires :

Gants en caoutchoucGants en caoutchouc
Thermomètre de laboratoireThermomètre de laboratoire
3

Pour the next layer and cover

Pour a second 1/2 inch layer on the first. Lower the top glass plate onto it so it rests on the syrup and keeps pressing on it. Leave another 24 hours at about 20 °C. For a thicker block repeat the layers, a day apart, and put the plate on the last one.

Outils nécessaires :

VitreVitre
4

Heat at 80 °C

Take the glass sandwich out of the frame and heat it for three hours at 80 °C to finish the polymerisation.

Outils nécessaires :

Étuve de séchageÉtuve de séchage
Thermomètre de laboratoireThermomètre de laboratoire
Gants résistants à la chaleurGants résistants à la chaleur
5

Spring off the glass

Spring the glass plates off the block with a knife blade. Both faces come out smooth and polished.

Outils nécessaires :

Cutter de précisionCutter de précision
Gants en caoutchoucGants en caoutchouc

Matériaux

1

Outils requis

9

Blueprints liés

Ces blueprints partagent des connaissances — techniques, matériaux ou principes

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...