Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Intermédiaire
30-60 minutes per charge

Consignes

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Matériaux pour cette étape :

Minerai de bismuth natifMinerai de bismuth natif1 12 cwt per tube charge

Outils nécessaires :

MarteauMarteau
Bascule industrielle à plateformeBascule industrielle à plateforme
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Matériaux pour cette étape :

Charbon de boisCharbon de bois1 powdered, in the pots and for the pot fire

Outils nécessaires :

Four de liquation du bismuthFour de liquation du bismuth
Creuset en fonteCreuset en fonte
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Matériaux pour cette étape :

Bois de chauffageBois de chauffage1 about 63 cu ft per 20 cwt of ore

Outils nécessaires :

Four de liquation du bismuthFour de liquation du bismuth
Tige de ferTige de fer
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Outils nécessaires :

Râteau en ferRâteau en fer
Four de liquation du bismuthFour de liquation du bismuth
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Outils nécessaires :

Creuset en fonteCreuset en fonte
Poche de fonderiePoche de fonderie
LingotièreLingotière

Matériaux

3

Outils requis

8

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...