Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper
Charlie

Créé par

Charlie

18. octobre 2026DE
11
0
0
0
0

Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper

Bromide paper is paper coated with silver bromide in gelatin, the printing and enlarging paper of the darkroom. Thorpe (1913) gives a beginner's emulsion: gelatin swelled in potassium bromide solution, silver nitrate made clear with strong ammonia, the two joined under ruby light, ripened, set, washed, and spread on paper as on a glass plate. From the moment the silver goes in, work only by ruby light. Grain and ounce figures are Thorpe's; the gram conversions and the 10-sheet batch are ours. The picture: our own drawing.
Avancé
4 days

Consignes

1

Swell the gelatin

Dissolve 185 grains (12.0 g) of potassium bromide in 5 oz (142 ml) of water. Cover 300 grains (19.4 g) of hard gelatin with it and stir until it softens and swells.

Matériaux pour cette étape :

Bromure de potassiumBromure de potassium12 g
Gélatine en poudreGélatine en poudre19.4 g

Outils nécessaires :

EauEau
Bécher en verreBécher en verre
Baguette de verreBaguette de verre
Balance à fléauBalance à fléau
2

Dissolve the silver

Dissolve 231 grains (15.0 g) of silver nitrate in 5 oz (142 ml) of water with gentle heat in the water bath. Add strong ammonia (0.880) a little at a time, stirring, until the precipitate that first forms dissolves again.

Matériaux pour cette étape :

Nitrate d'argentNitrate d'argent15 g

Outils nécessaires :

EauEau
Solution d'ammoniaque forte (0,880)Solution d'ammoniaque forte (0,880)
Bécher en verreBécher en verre
Baguette de verreBaguette de verre
Grande casserole (inférieure, pour bain-marie)Grande casserole (inférieure, pour bain-marie)
3

Melt the gelatin, never above 35 °C

Stand both vessels in the pan of water, never above 35 °C, stirring, until the gelatin is perfectly liquid. Up to here ordinary light is fine.

Outils nécessaires :

Grande casserole (inférieure, pour bain-marie)Grande casserole (inférieure, pour bain-marie)
ThermomètreThermomètre
Baguette de verreBaguette de verre
4

Add the silver under ruby light

From now on, ruby light only. Pour the silver solution into the gelatin in a thin stream, stirring all the time. Rinse the silver beaker with about 1 oz (28 ml) of warm water into the emulsion.

Outils nécessaires :

Lampe inactinique rubisLampe inactinique rubis
Bécher en verreBécher en verre
Baguette de verreBaguette de verre
EauEau
5

Ripen

Leave the emulsion in the hot water for half to three-quarters of an hour.

Outils nécessaires :

Grande casserole (inférieure, pour bain-marie)Grande casserole (inférieure, pour bain-marie)
Lampe inactinique rubisLampe inactinique rubis
6

Set in the dark

Pour it into a flat dish, put it in a light-tight box and let it set for at least 24 hours; two or three days is better.

Outils nécessaires :

Plateaux en céramique peu profondsPlateaux en céramique peu profonds
Boîte étanche à la lumièreBoîte étanche à la lumière
7

Wash through canvas

Scrape the set jelly onto wet coarse canvas and tie it into a bag. Knead it under water so it squeezes through in threads. Pour off the water, cover with fresh, wait 5 minutes and pour off: six to eight times.

Outils nécessaires :

SpatuleSpatule
Toile de cotonToile de coton
FicelleFicelle
EauEau
Lampe inactinique rubisLampe inactinique rubis
8

Drain and store

Turn the threads onto a strainer covered with a cloth and let the water drain. Rinse with methylated spirit and keep in a lidded jar until coating.

Outils nécessaires :

PassoirePassoire
MousselineMousseline
Alcool dénaturéAlcool dénaturé
Bocaux en verre avec couvercleBocaux en verre avec couvercle
Lampe inactinique rubisLampe inactinique rubis
9

Coat the paper

Melt the emulsion in the warm water bath. Lay a sheet of paper flat on a levelled glass slab. Pour emulsion on the middle to cover nearly half the sheet, and spread it to each end with a glass rod 2 inches wider than the sheet, held just off the surface.

Matériaux pour cette étape :

PapierPapier10 feuilles

Outils nécessaires :

Grande casserole (inférieure, pour bain-marie)Grande casserole (inférieure, pour bain-marie)
Feuille de verreFeuille de verre
Niveau à bulleNiveau à bulle
Baguette de verreBaguette de verre
Lampe inactinique rubisLampe inactinique rubis
10

Dry

When the coat has set, move the sheets to a rack in a drying box with a current of air. They dry in 12 to 48 hours. Keep them in the light-tight box.

Outils nécessaires :

SéchoirSéchoir
Boîte étanche à la lumièreBoîte étanche à la lumière

Matériaux

4

Outils requis

20

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...