Carbon Resistance Strip: Carbon and Phenolic Resin in Ethyl Acetate, Cured on Semi-Cured Phenolic Sheet

Podolsky (Wirt Company, US 2,060,114, 1936) bonded the carbon film into its base: the phenolic sheet is only half cured, the coating carries the same kind of resin, and its solvent (ethyl acetate) softens the sheet's surface. Heated calender rolls then finish the cure of sheet and coating together, so the track is hard, does not rub off and lasts. Cut across, the sheet gives resistance strips for a variable resistor. The picture: our diagram.
Intermédiaire
1 day

Consignes

1

Mix 21 carbon, 26 resin, 53 solvent

Make a solution of 21 % carbon, 26 % phenol-formaldehyde resin and 53 % ethyl acetate. The patent says the exact proportions are not essential; this is its example.

Matériaux pour cette étape :

CarboneCarbone21 parts
Bakélite liquide (produit de condensation phénol-formaldéhyde)Bakélite liquide (produit de condensation phénol-formaldéhyde)26 parts

Outils nécessaires :

Acétate d'éthyleAcétate d'éthyle
Balance à fléauBalance à fléau
Bécher en verreBécher en verre
AgitateurAgitateur
Masque respiratoire completMasque respiratoire complet
Gants en caoutchoucGants en caoutchouc
2

Coat the semi-cured sheet

Use a phenolic sheet whose cure was stopped before it fully hardened. A roller turning in a pan of the solution coats its underside.

Matériaux pour cette étape :

Feuille phénolique semi-polymériséeFeuille phénolique semi-polymérisée1 pièce

Outils nécessaires :

Paire de rouleaux d'enduction par trempagePaire de rouleaux d'enduction par trempage
Masque respiratoire completMasque respiratoire complet
Gants en caoutchoucGants en caoutchouc
3

Cure between calender rolls at 350 °F

Pass the coated sheet between calender rolls heated to about 350 °F (177 °C). This finishes the cure and bonds the coating to the sheet. The patent sometimes calenders it again to burnish the surface.

Outils nécessaires :

Cylindres de calandre chauffésCylindres de calandre chauffés
Gants résistants à la chaleurGants résistants à la chaleur
4

Cut into strips

Cut the sheet across into strips of the width wanted. Ours: tin snips.

Outils nécessaires :

Cisaille à tôleCisaille à tôle
Gants en caoutchoucGants en caoutchouc

Matériaux

3

Outils requis

10

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...