Carbon Steel Strip: Saw Plate Sheared and Annealed Soft
Forge

Créé par

Forge

26. octobre 2026NO
11
0
0
0
0

Carbon Steel Strip: Saw Plate Sheared and Annealed Soft

Thin carbon steel strip, soft enough to punch, file and score: the stock for utility-knife blades, hacksaw blades and hole saws, which are hardened only after they are shaped. Start from crucible steel rolled to gauge, cut it into strips with plate shears, then anneal it the way Harcourt's Elementary Forge Practice (1920) gives for tool steel: cherry red, about 1400 °F, and buried in perfectly dry ashes until cold. Cutting strips instead of saw outlines and the file test are ours. The picture is our drawing.
Débutant
1 day (cooling overnight)

Consignes

1

Roll the plate

Roll crucible steel to the gauge the blades need, as in this blueprint. Stop before the saw outlines are sheared.
2

Mark the strips

Scribe lines along the plate, one strip width apart. The width is whatever the blades need (ours).

Matériaux pour cette étape :

Tôle d'acier pour lames de scieTôle d'acier pour lames de scie1 pièce

Outils nécessaires :

Pointe à tracerPointe à tracer
Règle de contrôleRègle de contrôle
3

Shear into strips

Cut along the lines with plate shears, as Grimshaw's saw plates are cut to outline after rolling.

Outils nécessaires :

Cisaille à tôleCisaille à tôle
4

Fill a bucket with dry ash

Fill an iron bucket with ashes. They must be perfectly dry, so they conduct heat poorly and the steel cools slowly. Dry slaked lime also works.

Outils nécessaires :

Cendre de bois durCendre de bois dur
Seau métalliqueSeau métallique
5

Heat to cherry red

Heat the strips evenly in the forge to a cherry red, about 1400 °F (760 °C). No hotter: overheated steel goes coarse in the grain and weak.

Outils nécessaires :

Forge de forgeronForge de forgeron
Pinces de forgeronPinces de forgeron
Gants de soudeurGants de soudeur
6

Bury and leave until cold

Bury the strips in the ash at once and leave them until they are entirely cold, overnight. The slower they cool, the softer they are.

Outils nécessaires :

Pinces de forgeronPinces de forgeron
Seau métalliqueSeau métallique
Gants de soudeurGants de soudeur
7

Check it is soft

Brush off the ash and stroke a corner with a file: it should bite easily. If it skates, anneal again (our test).

Outils nécessaires :

Lime à métauxLime à métaux

Matériaux

1

Outils requis

9

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.