Metal Electrode Arc Welding
Carbon arc welding needs two hands: one holds the arc, the other feeds filler wire into the pool. The improvement is almost embarrassingly simple once stated — make the electrode out of the filler. Now the rod that carries the arc also melts into the joint, one hand does the work of two, and the metal crosses the arc as fine droplets rather than being pushed in cold from the side.
Charles L. Coffin patented it as US 428,459, “Process of Welding Metals Electrically”, granted 20 May 1890. It is the first verifiable patent for metal-electrode arc welding, and it describes the transfer directly: metal is carried across the arc from the electrode to the work.
Priority is not the same as patent, and this blueprint says so. Nikolay Gavrilovich Slavyanov demonstrated a consumable metal electrode at Perm in 1888, two years earlier, casting metal into a mould with the arc. No citable patent number for that work could be verified from any source, so the blueprint is built on the document that exists and credits the man who was first. Function is the payload; attribution is metadata, and both are reported honestly.
The experiment below is a measurement, not a weld: you will weigh the electrode before and after and prove that the missing mass is now in the joint.
Consignes
Read the safety step first
Read the safety step first
Read step 12 before striking anything. Arc ultraviolet injures eyes faster than you can decide to look away.
Outils nécessaires :
Notebook and PencilWeigh the electrode to 0.01 g
Weigh the electrode to 0.01 g
Weigh a single bare steel electrode. Record the mass. This number is the whole experiment.
Matériaux pour cette étape :
Metal Electrode Set1 pièceOutils nécessaires :
Digital Scale (0.01g)Weigh the test coupon
Weigh the test coupon
Clean a steel flat bar coupon with 220 grit until bright, then weigh it. Rust and scale would falsify the mass balance.
Matériaux pour cette étape :
Mild Steel Flat Bar1 pièce
Sandpaper (220 Grit)1 feuilleOutils nécessaires :
Digital Scale (0.01g)Set the work on firebrick and clamp the return
Set the work on firebrick and clamp the return
Lay the coupon on firebrick. Clamp the return lead to the coupon itself, not to the bench.
Matériaux pour cette étape :
Mild Steel Flat Bar1 pièce
Firebricks2 piècesOutils nécessaires :
C-ClampGear up and check the helmet
Gear up and check the helmet
Auto-darkening helmet, leather gloves, covered arms. Test the lens before striking.
Outils nécessaires :
Auto-Darkening Welding Helmet
Leather GlovesRun a single short bead
Run a single short bead
Strike by scratching, hold a short arc, and run one 40 mm bead along the coupon at a steady pace. Stop. Do not chase a second pass.
Matériaux pour cette étape :
Metal Electrode Set1 pièce
Mild Steel Flat Bar1 pièceOutils nécessaires :
Auto-Darkening Welding HelmetLet everything cool, then re-weigh both
Let everything cool, then re-weigh both
Cool to room temperature. Weigh the remaining electrode stub and the coupon again. Record both.
Outils nécessaires :
Digital Scale (0.01g)Do the mass balance
Do the mass balance
Electrode lost, coupon gained. Compare the two numbers. The coupon gains less than the electrode loses — the difference left as spatter and oxide.
Matériaux pour cette étape :
Graph Paper1 feuilleOutils nécessaires :
Notebook and PencilCalculate the deposition efficiency
Calculate the deposition efficiency
Divide the coupon's gain by the electrode's loss and multiply by 100. That percentage is deposition efficiency, a number every welding consumable is still sold on.
Matériaux pour cette étape :
Graph Paper1 feuilleOutils nécessaires :
Notebook and PencilMeasure the bead and find the spatter
Measure the bead and find the spatter
Measure bead width and length with the caliper. Look at the plate around the bead: the scattered beads of frozen metal are the missing mass.
Outils nécessaires :
Vernier Caliper
Magnifying GlassRecord what a bare electrode cannot do
Record what a bare electrode cannot do
Note the bead's appearance: porous, dark, irregular. Nothing protected the pool from the air. Kjellberg fixes this seventeen years later.
Matériaux pour cette étape :
Notebook and Pencil1 pièceSafety awareness — arc eye and fume
Safety awareness — arc eye and fume
An electric arc emits ultraviolet light strong enough to burn the cornea in seconds. The injury is called photokeratitis, or “arc eye”. It is not felt at the time — the pain arrives six to twelve hours later, typically in the middle of the night, and feels like sand under the eyelids. It normally heals in a day or two, but repeated exposure is cumulative.
Nobody in the room may look at an arc unshielded, including bystanders. Ordinary safety glasses do not protect against it and neither does a quick glance. Use an auto-darkening helmet, screen the work so passers-by cannot see it, and warn anyone nearby before striking. The same ultraviolet burns exposed skin like strong sunburn, so cover arms and neck.
Fume. Arc welding steel makes a metal-oxide smoke that should never be breathed. Ventilate, keep your head out of the plume, and use plain mild steel only — galvanised coatings release zinc oxide and cause metal fume fever.
Hot metal has no colour. Steel stops glowing at around 500 °C and is still hot enough to cause an immediate deep burn. Assume anything you have welded is hot until measured otherwise.
Outils nécessaires :
Auto-Darkening Welding Helmet
Leather Gloves
Infrared ThermometerHistory & Context
History & Context
US 428,459, “Process of Welding Metals Electrically”, Charles L. Coffin, granted 20 May 1890. Coffin, of Detroit, is the first person to hold a verifiable American patent for using a metal electrode that is itself consumed into the joint.
Slavyanov came first and this blueprint says so. Nikolay Gavrilovich Slavyanov (1854-1897), chief of the Perm cannon works, demonstrated arc welding with a consumable metal electrode in 1888 and used it to repair castings and to cast metal directly in a mould under the arc. He also introduced a molten-slag blanket over the pool — an idea that reappears in 1936 as submerged arc welding. What is missing is a patent number that any source could confirm. The honest position is that Slavyanov was first to the technique and Coffin was first to the document, and the blueprint prints both.
Why metal transfer changes everything. With a carbon electrode the filler arrives cold and unmixed. With a consumable electrode the metal crosses as droplets that have passed through the arc's own plasma, arriving superheated and alloyed. That is why consumable-electrode processes penetrate deeper at the same current, and why every dominant welding process today — stick, MIG, flux-cored, submerged arc — is a consumable electrode process. TIG, in 1942, is the deliberate exception.
What Coffin's bare rod could not solve. A bare electrode leaves the pool naked in the atmosphere. Nitrogen and oxygen dissolve into it, giving porosity, brittleness and a weld with perhaps half the parent metal's ductility. Almost every welding process developed after Coffin is, one way or another, an answer to that single problem.
Matériaux
6- 2 piècesEspace réservé
- 3 piècesEspace réservé
- 1 feuilleEspace réservé
- 2 piècesEspace réservé
- 2 feuillesEspace réservé
- 1 pièceEspace réservé
Outils requis
8- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Matériaux des Blueprints connectés
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.