Electrolytic Iron: Brown Ferrous Electrolyte, Rotating Cathode at 75-77 °C, Graphite Anodes (Bouchayer, US 1,516,326)
Iron plated out of a fresh green ferrous bath comes off rough and useless. Bouchayer first stirred the bath in air until it turned bright brown; the iron oxychloride formed takes care of the hydrogen at the cathode, and the deposit grows even and compact at high current.
Result: electrolytic iron, deposited at about 98 % current yield.
Source: Bouchayer, US 1,516,326 (1924). Not given: cathode material, purity of the iron. Picture drawn by Youblob.
Avancé
Factory process
Consignes
1
1
Make up the electrolyte at 20 °Bé
Make up the electrolyte at 20 °Bé
Dissolve ferrous sulfate in water (Bouchayer also allows ferrous chloride or a mix). Concentration: e.g. 20 °Bé, then keep it constant.
Matériaux pour cette étape :
Sulfate de fer1 as requiredOutils nécessaires :
Eau
Densimètre
Cuve d'électrolyse2
2
Stir it in air until brown
Stir it in air until brown
Agitate the green bath in air, e.g. by turning the anode, until it is bright brown and stops foaming. Used green, it gives only an irregular deposit.
Outils nécessaires :
Cuve d'électrolyse3
3
Circulate it through iron filings
Circulate it through iron filings
Pump the electrolyte through a mass of iron filings in a separate vessel; it takes back iron and forms the ferric hydroxide that keeps the bath working. Keep it moving fast past the anodes: this lowers the phosphorus.
Matériaux pour cette étape :
Limaille de fer1 as requiredOutils nécessaires :
Pompe à eau4
4
Deposit on a rotating cathode
Deposit on a rotating cathode
Electrolyse between graphite anodes and a rotating cathode. Temperature: e.g. 75-77 °C at 1000 A/m², held exactly constant and below boiling; cathode speed: e.g. 120 m/min at 800 A/m². Cathode material: not given.
Outils nécessaires :
Électrode en graphite
Alimentation en courant continu
Thermomètre
Cuve d'électrolyse5
5
Strip and reheat the deposit
Strip and reheat the deposit
Take the compact iron deposit off the cathode; it is usable after a slight reheating (temperature not given).
Outils nécessaires :
Cuve d'électrolyseMatériaux
2- 1 as requiredEspace réservé
- 1 as requiredEspace réservé
Outils requis
7- Espace réservé
- Espace réservé
- Espace réservé
- 1 vendor sell this, none ship to you yetEspace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Ce plan fabrique
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes