Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 75 °C (McIntire, Dow 1948, Ex. 3, Test 4)
Charlie

Créé par

Charlie

28. octobre 2026DE
1
0
0
0
0

Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 75 °C (McIntire, Dow 1948, Ex. 3, Test 4)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 75 °C (395 psi in the tower), it swelled into a log 18 to 20 inches across, weighing 2.9 lb per cubic foot, with uniform cells finer than at 60 °C. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Avancé
3 days

Consignes

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Matériaux pour cette étape :

PolystyrènePolystyrène300 livres

Outils nécessaires :

Réacteur sous pressionRéacteur sous pression
Balance à fléauBalance à fléau
Gants en caoutchoucGants en caoutchouc
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Matériaux pour cette étape :

PropylènePropylène100 livres

Outils nécessaires :

Bouteille de gaz sous pressionBouteille de gaz sous pression
Réacteur sous pressionRéacteur sous pression
Lunettes-masque anti-projections chimiquesLunettes-masque anti-projections chimiques
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Outils nécessaires :

Réacteur sous pressionRéacteur sous pression
Thermomètre de laboratoireThermomètre de laboratoire
4

Let it out at 75 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 75 °C. The pressure is about 395 psi. The gel flows out and swells into a log 18 to 20 inches across, 2.9 lb per cubic foot, with uniform cells finer than at 60 °C. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Outils nécessaires :

Réacteur sous pressionRéacteur sous pression
Thermomètre de laboratoireThermomètre de laboratoire
Lunettes-masque anti-projections chimiquesLunettes-masque anti-projections chimiques
Gants en caoutchoucGants en caoutchouc
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Outils nécessaires :

Scie de menuisierScie de menuisier
Gants en caoutchoucGants en caoutchouc

Matériaux

2
  • 300 livres
    Espace réservé
  • 100 livres
    Espace réservé

Outils requis

7

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...