Fired Silver Paint: Silver Oxide and Flux in Polyvinyl Alcohol and Water (Gray, Erie Resistor 1954, Ex. 2)
A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in polyvinyl alcohol dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. Gray found this paint so stable that it kept six months.
Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 2. Not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
Débutant
1 day
Consignes
1
1
Dissolve 2 g polyvinyl alcohol in the water
Dissolve 2 g polyvinyl alcohol in the water
For 100 g of paint: dissolve 2 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 34 to 44 g. Warming is ours.
Matériaux pour cette étape :
Alcool polyvinylique en poudre2 g
Eau distillée1 as requiredOutils nécessaires :
Balance à fléau
Bécher en borosilicate
Plaque chauffante
Baguette en verre borosilicaté2
2
Grind in silver oxide and flux
Grind in silver oxide and flux
Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.
Matériaux pour cette étape :
Oxyde d'argent50 g
Sous-nitrate de bismuth1 as requiredOutils nécessaires :
Balance à fléau
Mortier et pilon
Gants en nitrile3
3
Add 2 to 4 g alcohol against foam
Add 2 to 4 g alcohol against foam
Stir in 2 to 4 g ethyl alcohol. It stops the polyvinyl alcohol from foaming.
Matériaux pour cette étape :
Éthanol de laboratoire, 95 %1 as requiredOutils nécessaires :
Baguette en verre borosilicaté4
4
Store
Store
Keep it in a closed jar. Gray found no reaction between the ingredients in six months, and the paint can stand for some hours in use without stirring.
Outils nécessaires :
Bocaux en verre teinté à fermeture hermétiqueMatériaux
5- Espace réservé
- 1 as requiredEspace réservé
- 50 gEspace réservé
- 1 as requiredEspace réservé
- 1 as requiredEspace réservé
Outils requis
7- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Ce plan fabrique
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.