Lead Came: Window Rods Cast in a Split Wooden Mould (Theophilus, tr. Hendrie 1847)
Forge

Créé par

Forge

4. novembre 2026NO
12
0
0
0
0

Lead Came: Window Rods Cast in a Split Wooden Mould (Theophilus, tr. Hendrie 1847)

Theophilus' way to cast window leads without an iron mould: a stick of fir is split, a groove marked with a red-dyed flax thread and cut along both halves, the halves bound with a strap and the lead poured in again and again until the hot lead has burnt the groove to the bottom. Each rod is then trimmed in a slotted wooden gauge, cut with a knife on both sides and scraped smooth. Source: Theophilus, De Diversis Artibus, Book II, ch. XXVI, tr. R. Hendrie (1847), pp. 149-151. Picture: p. 151.
Intermédiaire
Unknown

Consignes

1

Split and mark the wood

Take fir or another wood that splits smoothly, the size of the iron mould (a yard long, two fingers broad, a finger thick). Split it and round the outside. Mark each end of both pieces for the width of the rod. Stretch a thin twisted flax thread wet with red colour from mark to mark on one inner face and press the other piece against it, so the line shows on both; do the same for the second line.

Outils nécessaires :

Moule à plombs de vitrailMoule à plombs de vitrail
Fil de linFil de lin
Cutter de précisionCutter de précision
2

Cut the groove

Cut the groove between the lines with a knife, as wide and deep as you wish, but not through the lower end; leave an opening at the top for pouring.

Outils nécessaires :

Cutter de précisionCutter de précision
Moule à plombs de vitrailMoule à plombs de vitrail
3

Cast the rods

Melt the lead as for the iron mould. Bind the two halves together with a strap from top to bottom, hold the mould with a wooden holder and pour in the lead; loosen the strap and take out the rod. Bind and cast again until the burning reaches the bottom of the groove; after that you can cast gently as many as you wish.

Matériaux pour cette étape :

Lingot de plombLingot de plomb1 pure lead

Outils nécessaires :

Moule à plombs de vitrailMoule à plombs de vitrail
Lanière de cuirLanière de cuir
Pot en terre cuitePot en terre cuite
Charbon de boisCharbon de bois
LoucheLouche
4

Trim the rods

Cut a piece of wood two fingers wide and as thick as the inside of the groove, split in the middle at one end so the rod fits into the slit. With the rod in it, cut it with a knife on both sides, then smooth and scrape it as you like.

Outils nécessaires :

Cutter de précisionCutter de précision

Matériaux

1

Outils requis

7

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...