Measuring the Coating: The Average Is Not the Minimum
A plated layer is usually a few microns thick — too thin to see, too thin for a rule, and thin enough that a specification is written in microns at the worst point.
It is nevertheless easy to measure, in several independent ways, and the ways disagree for an informative reason: **weighing gives the average over the whole part, and the specification is about the thinnest place.** The previous rung explains why those two numbers can differ by a factor of several.
So both measurements are needed, and they answer different questions: the weight checks the process, and the thin spot checks the part.
Intermédiaire
2 hours
Consignes
1
1
By weight, which needs only a balance
By weight, which needs only a balance
**Weigh dry, before and after.** The gain is the metal deposited, and with the area and the density that is an average thickness directly.
**Clean and dry the part fully both times.** Water in a recess weighs more than the coating does, which is the commonest error in this measurement.
**Weigh by difference on the same balance**, in the same session if possible. A systematic error that is the same both times cancels; changing balances between the two weighings does not.
**The area must be right.** An area underestimated by 20% gives a thickness overestimated by 20%, and it is the larger source of error than the balance.
**It is also how current efficiency is measured**, by comparing the gain with Faraday's prediction, so one careful weighing calibrates the whole bath.
**It cannot see distribution at all.** A part with half its area at 20 microns and half at nothing weighs exactly the same as one evenly at 10.
Matériaux pour cette étape :
Plaque d'acier doux2 pièces
Eau distillée1 pièceOutils nécessaires :
Balance de précision
Pied à coulisse numérique 6 pouces2
2
The arithmetic, and what a balance can resolve
The arithmetic, and what a balance can resolve
Chargement du notebook Jupyter…
Outils nécessaires :
Ordinateur de bureau3
3
The other ways, and what each one can see
The other ways, and what each one can see
**Micrometer, before and after.** Works on a flat part for coatings above a few microns, and it measures the specific spot it is placed on — which is its advantage over weighing. It cannot resolve a 1 micron coating, because the instrument's own repeatability is of that order.
**Magnetic gauge.** A magnet is pulled away from the surface and the force measured; a non-magnetic coating on a magnetic substrate holds the magnet further away. Non-destructive, instant, cheap, and the standard method for zinc or nickel on steel.
**Eddy current gauge.** The same idea for a non-conductive coating on a non-magnetic metal — anodising on aluminium, mainly.
**Cross-section under a microscope.** Cut, mount, polish and etch, then measure the layer directly with a calibrated eyepiece. Destructive, slow, and definitive — it shows the thickness at every point across the section, plus the structure of the deposit and any porosity.
**Coulometric stripping.** Dissolve the coating anodically from a known small area and count the charge it takes. Faraday's law run backwards. Accurate to a fraction of a micron, destroys a small spot, and it is the reference method.
**Pick the method for the question.** Process control: weigh. A specification at a point: a gauge. A dispute: a cross-section.
Matériaux pour cette étape :
Plaque d'acier doux1 pièce
Feuille de nickel1 pièceOutils nécessaires :
Micromètre
Balance de précision
Loupe de bijoutier4
4
Porosity, which thickness does not measure
Porosity, which thickness does not measure
A barrier coating protects only if it is continuous. A nickel layer of the right average thickness with pores through it protects the substrate worse than no coating at all, because the tiny exposed area at the bottom of each pore corrodes at an accelerated rate against the large noble cathode around it.
**The ferroxyl test** finds pores in a coating on steel. A gel or paper soaked in potassium ferricyanide and sodium chloride is laid on the surface; wherever iron is exposed, a bright Prussian blue spot appears within minutes. The pattern of spots is the pattern of pores.
**A salt spray test** is the accelerated corrosion standard: hours to failure in a controlled salt fog. It correlates loosely with service life and it is what specifications quote, because it is repeatable.
**Pores come from** a substrate that was not smooth, gas bubbles that clung during plating, particles in the bath, and too thin a deposit — porosity falls sharply with thickness, which is the real reason minimum thicknesses are specified.
**This is also why decorative chrome is always over nickel.** The chromium is a third of a micron and unavoidably porous; the nickel underneath is ten microns and is what actually protects. A chrome-plated part that has rusted has usually had its nickel skimped, not its chrome.
Matériaux pour cette étape :
Plaque d'acier doux2 piècesOutils nécessaires :
Loupe de bijoutier
Bécher en borosilicateMatériaux
3- 2 piècesEspace réservé
- 1 pièceEspace réservé
- 1 pièceEspace réservé
Outils requis
6- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.