Polypropylene Felt: a Spunbonded Web, Kinney 1967
Tex

Créé par

Tex

18. octobre 2026FO
11
0
0
0
0

Polypropylene Felt: a Spunbonded Web, Kinney 1967

A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live. The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
Avancé
1 day

Consignes

1

Melt and spin

Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.

Matériaux pour cette étape :

Granulés de polypropylèneGranulés de polypropylène500 g

Outils nécessaires :

Extrudeuse de plastiqueExtrudeuse de plastique
Filière de filageFilière de filage
PyromètrePyromètre
Balance à fléauBalance à fléau
Gants en cuirGants en cuir
2

Quench

Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.

Outils nécessaires :

Compresseur d'airCompresseur d'air
3

Draw with the air jet

Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.

Outils nécessaires :

Buse d'étirage à airBuse d'étirage à air
Compresseur d'airCompresseur d'air
ManomètreManomètre
4

Charge the filaments

8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.

Outils nécessaires :

Unité de charge coronaUnité de charge corona
5

Lay the web

Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.

Outils nécessaires :

Table de déposeTable de dépose
6

What you get

An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.

Outils nécessaires :

Balance à fléauBalance à fléau

Matériaux

1

Outils requis

10

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...