Polystyrene: Styrene Polymerised by Heat Alone in Sealed Tubes
Charlie

Créé par

Charlie

20. octobre 2026DE
12
0
0
0
0

Polystyrene: Styrene Polymerised by Heat Alone in Sealed Tubes

Polystyrene is styrene joined into long chains: a tough, glass-clear solid. Heat alone does it. Ostromislensky (US 1,683,402, 1928) sealed pure styrene in glass tubes and held them at 140 °C for 20 hours; hotter goes faster (155 °C 18 h, 165 °C 16 h), but at 175 °C another, unwanted form starts to appear. As it cools the polystyrene shrinks away from the glass and usually breaks the tube. The picture: our diagram.
Intermédiaire
1 day

Consignes

1

Fill and seal the tubes

Use styrene of 92 % purity or better. Fill glass tubes about 0.7 cm wide and 26 cm long to about 4.5 cm (a sixth of the tube) and seal them. Ours: seal in a torch flame (the patent does not say how).

Matériaux pour cette étape :

StyrèneStyrène4.5 ml

Outils nécessaires :

Kit de tubes en verreKit de tubes en verre
Chalumeau à propaneChalumeau à propane
Lunettes-masque anti-projections chimiquesLunettes-masque anti-projections chimiques
Gants en caoutchoucGants en caoutchouc
Sorbonne (à extraction)Sorbonne (à extraction)
2

Heat at 140 °C for 20 hours

Stand the tubes upright with their lower part in an air bath at about 140 °C for 20 hours (ours: a drying oven). Shorter at higher heat: 155 °C 18 h or 165 °C 16 h. Do not go above 175 °C.

Outils nécessaires :

Étuve de séchageÉtuve de séchage
Thermomètre de laboratoireThermomètre de laboratoire
3

Cool and break out

Let the tubes cool. The polystyrene comes away from the glass and usually breaks it. Remove the glass and break the clear solid into small pieces: it is very tough and hard to grind.

Outils nécessaires :

Gants résistants à la chaleurGants résistants à la chaleur
Lunettes-masque anti-projections chimiquesLunettes-masque anti-projections chimiques

Matériaux

1
  • 4.5 ml
    Espace réservé

Outils requis

8

Blueprints liés

Ces blueprints partagent des connaissances — techniques, matériaux ou principes

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...