Precipitated Silver: Silver Chloride Reduced by Zinc in Acidulated Water (Thorpe 1913)

Fine silver powder without melting anything. Hydrochloric acid throws silver out of solution as white silver chloride. Zinc in slightly acid water then takes the chlorine away and leaves the silver as a grey powder. Source: Thorpe, Dictionary of Applied Chemistry, vol. 4 (1913), Silver. Thorpe gives no amounts, times or end-point. Ours: a silver nitrate solution, zinc sheet strips, hydrochloric acid of the two acids he names, and the washing and drying. Picture drawn by Youblob.
Débutant
1 day

Consignes

1

Dissolve silver nitrate in water

Ours: dissolve silver nitrate in distilled water as the silver solution. Silver nitrate stains and burns skin: gloves and goggles.

Matériaux pour cette étape :

Nitrate d'argentNitrate d'argent1 as required
Eau distilléeEau distillée1 as required

Outils nécessaires :

Bécher en borosilicateBécher en borosilicate
Baguette en verre borosilicatéBaguette en verre borosilicaté
Gants en nitrileGants en nitrile
Lunettes-masque anti-projections chimiquesLunettes-masque anti-projections chimiques
2

Throw down silver chloride with hydrochloric acid

Add hydrochloric acid to the solution. White silver chloride falls. Ours: add it while it still makes a precipitate, let it settle and pour off the liquid.

Matériaux pour cette étape :

Acide chlorhydriqueAcide chlorhydrique1 as required

Outils nécessaires :

Bécher en borosilicateBécher en borosilicate
Baguette en verre borosilicatéBaguette en verre borosilicaté
Gants en nitrileGants en nitrile
Lunettes-masque anti-projections chimiquesLunettes-masque anti-projections chimiques
3

Reduce the chloride with zinc in acid water

Cover the chloride with water made slightly acid with hydrochloric acid (Thorpe: hydrochloric or sulphuric) and put zinc in it. The zinc reduces the chloride to silver. Ours: strips of zinc sheet, left in until no white chloride is left. Time not given.

Matériaux pour cette étape :

Feuille de zincFeuille de zinc1 as required
Acide chlorhydriqueAcide chlorhydrique1 as required
Eau distilléeEau distillée1 as required

Outils nécessaires :

Bécher en borosilicateBécher en borosilicate
Baguette en verre borosilicatéBaguette en verre borosilicaté
Gants en nitrileGants en nitrile
Lunettes-masque anti-projections chimiquesLunettes-masque anti-projections chimiques
4

Take out the zinc, wash and dry the silver

Ours: lift out what is left of the zinc, wash the grey silver powder with water until the washings are no longer acid, filter, and dry it. Keep it in a closed jar.

Outils nécessaires :

Eau distilléeEau distillée
Papier filtrePapier filtre
Étuve de séchageÉtuve de séchage
Bocal en verreBocal en verre

Matériaux

4

Outils requis

8

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...