Rabbit Skin Glue Granules
Animal glue is made by boiling skins until their collagen dissolves. Rabbit-skin glue dries more flexible than most hide glues, so painters size and prime canvas with it, and bookbinders and gesso makers use it. Soak the skins, warm them in water to about 70 °C, draw off the glue liquor, let it set, then dry it and break it into granules that keep for years if kept dry.
The picture: rabbit-skin glue granules (left) and granules swelling in water (right).
Débutant
A week, mostly drying
Consignes
1
1
Soak the skins
Soak the skins
Cut the skins into small pieces and soak them in cold water until soft. Glue works treat hides with lime at this stage and then rinse and neutralise it; we leave the lime out, as in our hide-glue blueprint.
Matériaux pour cette étape :
Peaux de lapin500 g
Eau5 litresOutils nécessaires :
Seau
Cutter2
2
Rinse
Rinse
Pour off the soaking water and rinse the pieces in fresh water until it runs clear.
Matériaux pour cette étape :
Eau5 litresOutils nécessaires :
Seau3
3
Draw the glue
Draw the glue
Cover the pieces with water and hold it at about 70 °C for some hours. Pour the glue liquor off through a cloth. Add fresh water and repeat a little hotter each time.
Matériaux pour cette étape :
Eau4 litresOutils nécessaires :
Chaudron
Thermomètre
Étamine
Seau4
4
Let it set
Let it set
Pour the liquor in a thin layer on a cool, wet stone. As it cools it sets to a firm jelly.
Outils nécessaires :
Dalle de pierre plate5
5
Dry and break up
Dry and break up
Cut the jelly into small cubes and dry them on a rack in moving air until hard and glassy. Break them into granules and store them dry.
Outils nécessaires :
Cutter
Séchoir6
6
Melt for use
Melt for use
Soak granules in cold water until swollen, then warm in a double boiler and use warm, around 60 °C.
Matériaux pour cette étape :
Eau0.5 litreOutils nécessaires :
Bain-marie
Thermomètre7
7
Yield and strength
Yield and strength
Chargement du notebook Jupyter…
Ce plan fabrique
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.