Silicone Rubber Compound: Dimethyl Silicone Oil Gelled with Ferric Oxide, Agens 1948

Dimethyl silicone oil mixed with three-quarters its weight of red ferric oxide and a little aluminium chloride, heated to 130 °C, thins and then sets to a solid mass; milled on warm rubber rolls it becomes a silicone rubber compound ready to mould or extrude (Agens, General Electric, US 2,448,756, 1948). Cured, it stretches over 100 % and stays flexible at −60 °C. The picture: our drawing of the beaker, the mill and the sheet.
Avancé
A day

Consignes

1

Weigh the mix

To 400 g silicone oil add 300 g ferric oxide (75 % of the oil) and 5 g anhydrous aluminium chloride (1.25 %). Stir it smooth. Keep the chloride dry; it fumes in damp air.

Matériaux pour cette étape :

Huile de diméthylsiliconeHuile de diméthylsilicone400 g
Poudre de rouge à polir finePoudre de rouge à polir fine300 g

Outils nécessaires :

Chlorure d'aluminium (anhydre)Chlorure d'aluminium (anhydre)
Bécher en borosilicateBécher en borosilicate
AgitateurAgitateur
Balance de cuisine numériqueBalance de cuisine numérique
Gants en caoutchoucGants en caoutchouc
2

Heat to 130 °C

Heat the mix to 130 °C. It first gets thinner, then thickens fast until the whole mass is solid.

Outils nécessaires :

Plaque chauffantePlaque chauffante
ThermomètreThermomètre
Bécher en borosilicateBécher en borosilicate
3

Mill and sheet

Work the mass on rubber rolls at 125 °C for about half an hour and take it off as a sheet. This is the compound.

Outils nécessaires :

Mélangeur à cylindres pour caoutchoucMélangeur à cylindres pour caoutchouc
ThermomètreThermomètre
4

Test a piece

Agens's test: press a sheet about 1.3 mm thick between platens at 150 °C for ten minutes, then 15 minutes in an oven at 200 °C. It should stretch over twice its length.

Outils nécessaires :

Presse chauffante de moulage par compressionPresse chauffante de moulage par compression
Four de recuitFour de recuit
5

The mix

Chargement du notebook Jupyter…

Matériaux

2

Outils requis

10

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...