Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 3, 82 % iron, 3 % boron and 15 % neodymium by atoms: 7.0 MGOe. Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Expert
2 days

Consignes

1

Weigh sample 3: 82 Fe, 3 B, 15 Nd

Sample 3 is 82 % iron, 3 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 657.5 g iron, 24.7 g ferroboron, 319.3 g neodymium. Unknown: how these three are made.

Matériaux pour cette étape :

Fer électrolytiqueFer électrolytique657.5 g
FerroboreFerrobore24.7 g
Néodyme métalNéodyme métal319.3 g

Outils nécessaires :

Balance à fléauBalance à fléau
2

Melt by high frequency in argon and cast

Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.

Outils nécessaires :

Four à inductionFour à induction
Creuset en argile réfractaireCreuset en argile réfractaire
ArgonArgon
Bouteille de gaz sous pressionBouteille de gaz sous pression
Lingotière en cuivre refroidie à l’eauLingotière en cuivre refroidie à l’eau
Gants résistants à la chaleurGants résistants à la chaleur
3

Stamp to 35 mesh, ball-mill to 3-10 µm

Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.

Outils nécessaires :

BocardBocard
Jeu de tamis (mailles graduées)Jeu de tamis (mailles graduées)
Broyeur à boulets de ferBroyeur à boulets de fer
Lunettes de sécuritéLunettes de sécurité
4

Press in a 10 kOe field at 1.5 t/cm²

Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.

Outils nécessaires :

Presse sous champ magnétiquePresse sous champ magnétique
5

Sinter in argon at 1000-1200 °C

Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 3 measured 10.4 kG remanence, 1.8 kOe coercivity and 7.0 MGOe.

Outils nécessaires :

Four tubulaireFour tubulaire
ArgonArgon
Bouteille de gaz sous pressionBouteille de gaz sous pression
Gants résistants à la chaleurGants résistants à la chaleur
6

Magnetise the magnets

Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.

Outils nécessaires :

Méthode d’aimantation inconnueMéthode d’aimantation inconnue

Matériaux

3

Outils requis

14

Blueprints liés

Ces blueprints partagent des connaissances — techniques, matériaux ou principes

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...