Metal Oxide Varistor: Zinc Oxide with 0.2 % Bismuth Oxide, Sintered Disc (Masuyama 1972)
A non-linear resistor: the current through it rises far faster than the voltage across it. Masuyama, Matsuoka and Nishi made one from zinc oxide with a little bismuth oxide: pressed into a disc, sintered, lapped, and given metal electrodes. With 0.2 mole % bismuth oxide, sintered at 1000 °C and lapped to 1 mm, the disc measured a C-value of 43 at 1 mA and a nonlinearity exponent n of 4.3.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 1. Unknown: what the silver paint is. The patent calls the spraying and the paint well known. The spraying is ours, after US Army Corps of Engineers EM 1110-2-3401 (1999). The 10 g batch is our arithmetic. Picture: the patent's drawing.
Avancé
1 day
Consignes
1
1
Weigh 99.8 ZnO to 0.2 Bi2O3 and wet-mill 5 hours
Weigh 99.8 ZnO to 0.2 Bi2O3 and wet-mill 5 hours
Mix zinc oxide and bismuth oxide 99.8 : 0.2 by moles. Ours, for 10 g: 9.887 g zinc oxide and 0.113 g bismuth oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.
Matériaux pour cette étape :
Poudre d'oxyde de zinc9.887 g
Oxyde de bismuth0.113 gOutils nécessaires :
Balance à fléau
Broyeur à boulets de fer
Étuve de séchage2
2
Press discs 13 mm by 2.5 mm
Press discs 13 mm by 2.5 mm
Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm².
Outils nécessaires :
Presse hydraulique
Matrice de pressage de disques
Pied à coulisse3
3
Sinter 1 hour at 1000 °C and furnace-cool
Sinter 1 hour at 1000 °C and furnace-cool
Sinter the discs in air for 1 hour at 1000 °C, then let them cool in the furnace to room temperature (about 15-30 °C). Above 1200 °C the disc loses its nonlinearity.
Outils nécessaires :
Four à moufle4
4
Lap both faces to 1.0 mm
Lap both faces to 1.0 mm
Lap both faces with 600-mesh silicon carbide until the disc is 1.0 mm thick.
Outils nécessaires :
Pied à coulisse5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Ours, after US Army Corps of Engineers EM 1110-2-3401 (1999): wire-arc spray the aluminium from two 3.2 mm wires melted by an 18-40 V DC arc and atomised by compressed air, 15-20 cm from the disc and never at less than 45°, in at least two coats at right angles of 50-75 µm each. Unknown: the paint.
Matériaux pour cette étape :
Lingot d'aluminium1 as 3.2 mm spray wire
Peinture conductrice à l'argent1 as required
Fil de cuivre2 piècesOutils nécessaires :
Pied à coulisse
Pistolet de projection à l'arc électrique
Compresseur d'air industrielMatériaux
5- 9.887 gEspace réservé
- 0.113 gEspace réservé
- 1 as 3.2 mm spray wireEspace réservé
- 1 as requiredEspace réservé
- 2 piècesEspace réservé
Outils requis
10- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
- Espace réservé
Blueprints liés
Ces blueprints partagent des connaissances — techniques, matériaux ou principes
CC0 Domaine public
Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.
Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.