Acrylic Polymer Medium: Methyl Methacrylate Emulsified by Persulfate Alone
Charlie

Dibuat oleh

Charlie

20. Oktober 2026DE
10
0
0
0
0

Acrylic Polymer Medium: Methyl Methacrylate Emulsified by Persulfate Alone

Acrylic polymer medium is an emulsion of acrylic polymer in water, the binder of acrylic paint. ICI's Renfrew and Gates (US 2,296,403, 1942) found that a persulfate alone both keeps the monomer dispersed and starts it polymerising, so no soap is needed. Their Example 2 stirs 30 parts methyl methacrylate and 20 parts dibutyl phthalate (a plasticiser) hard in 100 parts water with 1 part persulfate at about 80 °C; the batch heats itself to 90-95 °C and gives a very stable emulsion. Using it as paint medium is our choice. The picture: our diagram.
Menengah
Half a day

Instruksi

1

Weigh the charge

Weigh 30 parts methyl methacrylate, 20 parts dibutyl phthalate, 100 parts water and 1 part persulfate (ours: potassium persulfate; the example used lithium persulfate, and the patent names potassium among the alternatives).

Material untuk langkah ini:

Metil MetakrilatMetil Metakrilat30 parts
Dibutil FtalatDibutil Ftalat20 parts
AirAir100 parts
Inisiator persulfatInisiator persulfat1 part

Alat yang dibutuhkan:

Neraca lenganNeraca lengan
Kacamata Pelindung Cipratan KimiaKacamata Pelindung Cipratan Kimia
Sarung tangan karetSarung tangan karet
2

Stir hard at about 80 °C

Put everything in a flask with a reflux condenser and stir very vigorously at about 80 °C, where it refluxes gently.

Alat yang dibutuhkan:

Labu alas bulatLabu alas bulat
Kondensor RefluksKondensor Refluks
PengadukPengaduk
Penangas AirPenangas Air
Pelat PemanasPelat Pemanas
Termometer LaboratoriumTermometer Laboratorium
Lemari asam (bersaluran buang)Lemari asam (bersaluran buang)
3

Let it heat itself

After about half an hour the polymerisation starts giving off heat and the temperature climbs to 90-95 °C on its own. Keep stirring.

Alat yang dibutuhkan:

PengadukPengaduk
Termometer LaboratoriumTermometer Laboratorium
4

Cool

When the temperature starts to fall, the polymerisation is complete. Stop stirring and let it cool. The result is a very stable emulsion.

Alat yang dibutuhkan:

Termometer LaboratoriumTermometer Laboratorium

Bahan

4

Alat yang Diperlukan

10

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.