Aqueous PTFE Dispersion: Tetrafluoroethylene Polymerised in Soapy Water (Berry 1951)
Charlie

Dibuat oleh

Charlie

28. Oktober 2026DE
1
0
0
0
0

Aqueous PTFE Dispersion: Tetrafluoroethylene Polymerised in Soapy Water (Berry 1951)

Ordinary soaps stop tetrafluoroethylene from growing into long chains. A fluorine soap does not: with 2 % of ammonium dodecafluoroheptanoate in the water, the gas polymerises into tiny PTFE ribbons that stay suspended. The result is a milky dispersion, a third of it polymer, the raw material for PTFE fine powder. Source: K. L. Berry (du Pont), US 2,559,752 (1951), Example III. Making the ammonium salt from our acid, and the apparatus, are ours. Picture drawn by Youblob.
Lanjutan
1 day

Instruksi

1

Make the ammonium salt

Ours: neutralise about 1.9 parts of dodecafluoroheptanoic acid with ammonia solution until just neutral to litmus, giving 2 parts of ammonium dodecafluoroheptanoate. Make it up with distilled water to 93 parts of water in all. Parts are by weight.

Material untuk langkah ini:

Asam dodekafluoroheptanoatAsam dodekafluoroheptanoat1.9 parts
Larutan amonia 25-28 %Larutan amonia 25-28 %1 as required to neutralise
Air SulingAir Suling93 parts

Alat yang dibutuhkan:

Kertas lakmusKertas lakmus
Wadah kacaWadah kaca
Neraca lenganNeraca lengan
2

Load the pressure vessel

Put the solution in a pressure vessel with 0.05 part of potassium persulfate and 5 parts of paraffin wax melting at 56–58 °C. The wax protects the colloid while it is stirred.

Alat yang dibutuhkan:

Inisiator persulfatInisiator persulfat
Lilin parafinLilin parafin
Reaktor bertekananReaktor bertekanan
Neraca lenganNeraca lengan
3

Heat and remove the air

Bring it to 80–85 °C, then evacuate the vessel and hold it under reduced pressure for several minutes to drive out air and dissolved oxygen.

Alat yang dibutuhkan:

Reaktor bertekananReaktor bertekanan
Pompa vakumPompa vakum
TermometerTermometer
4

Feed tetrafluoroethylene for 3.6 hours

Let in tetrafluoroethylene to 60 lb/sq in gauge. Agitate at 80–85 °C for 3.6 hours; each time the pressure falls to 55 lb/sq in, bring it back to 60.

Material untuk langkah ini:

TetrafluoroetilenaTetrafluoroetilena1 as required to hold 55–60 psi

Alat yang dibutuhkan:

Reaktor bertekananReaktor bertekanan
Tabung gas bertekananTabung gas bertekanan
Pengukur TekananPengukur Tekanan
TermometerTermometer
5

Cool and lift off the wax

Cool it. The paraffin sets on top and lifts off. Below it is a colloidal PTFE dispersion with 34 % solids.

Alat yang dibutuhkan:

Reaktor bertekananReaktor bertekanan
Toples Kaca BertutupToples Kaca Bertutup

Bahan

4

Alat yang Diperlukan

11

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...