Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate
Forge

Dibuat oleh

Forge

18. Oktober 2026NO
19
0
0
0
0

Bearing Steel Wire (52100): Drawn from Bar Through a Drawplate

Bearing balls are headed from thick wire of 52100 steel. Here 52100 bar is forged to rod and drawn through a drawplate. At 1 % carbon it is much harder than mild steel, so it is annealed soft before drawing and again after every two holes, using the 52100 anneal Verhoeven recommends. The picture: our drawing, bar to coil.
Lanjutan
2 days

Instruksi

1

Forge to rod

Heat the bar to a cherry-red heat and no hotter, and draw it out round on the anvil to a rod a little thicker than the drawplate's largest hole.

Material untuk langkah ini:

Batang baja bantalan (52100)Batang baja bantalan (52100)1 kg
ArangArang1 as required

Alat yang dibutuhkan:

Perapian pandai besiPerapian pandai besi
Landasan TempaLandasan Tempa
Palu kepala baji melintangPalu kepala baji melintang
Tang pandai besiTang pandai besi
Sarung tangan lasSarung tangan las
Kacamata pengamanKacamata pengaman
2

Anneal

In the oven, hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Alat yang dibutuhkan:

Oven perlakuan panasOven perlakuan panas
Termokopel dengan penampilTermokopel dengan penampil
Tang pandai besiTang pandai besi
Sarung tangan lasSarung tangan las
3

Clean and taper

Brush off all the scale, then file a long taper on the first 3 cm so it passes the first hole.

Alat yang dibutuhkan:

Set sikat kawatSet sikat kawat
Set KikirSet Kikir
Ragum MejaRagum Meja
4

Wax and draw

Clamp the drawplate in the vise. Wax the rod, push the taper through the first hole it does not slip through, and pull straight out with the draw tongs in one steady pull.

Material untuk langkah ini:

Malam LebahMalam Lebah20 g

Alat yang dibutuhkan:

Pelat tarik bajaPelat tarik baja
Tang tarikTang tarik
Ragum MejaRagum Meja
Sarung Tangan Kerja KulitSarung Tangan Kerja Kulit
5

Anneal every two holes

Draw through each next hole without skipping. After every two holes, coil the wire and anneal it again: hold it at 793 °C (1460 °F) for 30 minutes, cool in the oven no faster than 500 °C an hour to 682 °C (1260 °F), then cool in air.

Material untuk langkah ini:

Malam LebahMalam Lebah1 buah

Alat yang dibutuhkan:

Pelat tarik bajaPelat tarik baja
Tang tarikTang tarik
Oven perlakuan panasOven perlakuan panas
Termokopel dengan penampilTermokopel dengan penampil
6

Finish soft

Stop at the diameter your balls need, checked with the caliper, and give the coil a last anneal so it is soft for heading.

Alat yang dibutuhkan:

Jangka Sorong Digital 6 InciJangka Sorong Digital 6 Inci
Oven perlakuan panasOven perlakuan panas
Termokopel dengan penampilTermokopel dengan penampil
7

Troubleshooting

Bearing steel wire troubleshooting.

Flow

Loading...

Bahan

3

Alat yang Diperlukan

15

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...