The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Menengah
30-60 minutes per charge

Instruksi

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Material untuk langkah ini:

Bijih bismut murniBijih bismut murni1 12 cwt per tube charge

Alat yang dibutuhkan:

PaluPalu
Timbangan lantai industriTimbangan lantai industri
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Material untuk langkah ini:

ArangArang1 powdered, in the pots and for the pot fire

Alat yang dibutuhkan:

Tungku likuasi bismutTungku likuasi bismut
Kowi besiKowi besi
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Material untuk langkah ini:

Kayu BakarKayu Bakar1 about 63 cu ft per 20 cwt of ore

Alat yang dibutuhkan:

Tungku likuasi bismutTungku likuasi bismut
Batang besi bulatBatang besi bulat
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Alat yang dibutuhkan:

Garu besiGaru besi
Tungku likuasi bismutTungku likuasi bismut
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Alat yang dibutuhkan:

Kowi besiKowi besi
Gayung tuang logamGayung tuang logam
Cetakan batang logamCetakan batang logam

Bahan

3
  • 1 12 cwt per tube charge
    Placeholder
  • 1 powdered, in the pots and for the pot fire
    Placeholder
  • 1 about 63 cu ft per 20 cwt of ore
    Placeholder

Alat yang Diperlukan

8

Cetak biru ini membuat

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...