Gesso Sottile: Plaster of Paris Slaked a Month, Ground, Wrung and Tempered Warm with Parchment Size (Cennini, c. 1400)
Charlie

Dibuat oleh

Charlie

15. November 2026DE
7
0
0
0
0

Gesso Sottile: Plaster of Paris Slaked a Month, Ground, Wrung and Tempered Warm with Parchment Size (Cennini, c. 1400)

The fine gilding and painting ground of Cennino Cennini: plaster of Paris kept under water for a month, the water changed daily until it is dead and soft as silk, dried in cakes, then ground, wrung out in linen and tempered warm with size boiled from sheep-parchment shavings, never letting it boil or froth.
Menengah
A month of slaking, then an hour to temper

Instruksi

1

Slaking water

Memuat notebook Jupyter…
2

Read Cennini

"Kept moist in a large tub for at least a month; renew the water every day until it almost rots."
3

Slake the plaster

Put well-purified plaster of Paris in a large tub of water (the translator's note: about a gallon to each pound, so it cannot set). Keep it wet at least a month, changing the water every day, until it is completely slaked, all heat gone, and soft as silk.

Material untuk langkah ini:

Gips (Plaster of Paris)Gips (Plaster of Paris)1 buah
AirAir1 buah

Alat yang dibutuhkan:

Bak kayuBak kayu
4

Make cakes

Pour off the water (strain through linen), shape the paste into cakes and let them dry.

Alat yang dibutuhkan:

Kain linenKain linen
5

Boil the size

Boil shavings of sheep parchment in water until the water is down to one third. It is ready when a little rubbed between the palms makes one hand stick to the other. Strain it two or three times.

Material untuk langkah ini:

PerkamenPerkamen1 buah
AirAir1 buah

Alat yang dibutuhkan:

Panci berdinding tinggiPanci berdinding tinggi
Kain (Penyaring)Kain (Penyaring)
6

Grind and wring

Drop the cakes one by one into clean water and let them drink all they will. Grind a little at a time on the slab, adding no more water. Gather it on strong white linen until you have a loaf's worth, fold the cloth and wring out all the water you can.

Material untuk langkah ini:

AirAir1 buah

Alat yang dibutuhkan:

Periuk keramik berglasirPeriuk keramik berglasir
Lempeng Batu RataLempeng Batu Rata
Penggerus tanganPenggerus tangan
Kain linenKain linen
7

Temper warm

In a new, grease-free (better glazed) pipkin, scrape the gesso fine with a knife like cheese. Add the size, less than for gesso grosso, and work it with the hand like fritter batter so it does not froth. Stand the pipkin in a cauldron of very hot water to keep it warm: it must never boil.

Alat yang dibutuhkan:

Periuk keramik berglasirPeriuk keramik berglasir
PisauPisau
Kuali besarKuali besar
8

Troubleshooting

Gesso troubleshooting.

Flow

Loading...
9

History and honest limits

From Cennino Cennini, **Il Libro dell'Arte** (c. 1400), chaps. 113, 116-117, in Herringham's translation (1899), pp. 93-98 (checked on the archive.org scan bookartcenninoc01herrgoog). The water ratio is Herringham's footnote, not Cennini's. The smooth stone slab in place of porphyry and the metric figures are ours.

Bahan

3

Alat yang Diperlukan

9

CC0 Domain Publik

Cetak biru ini dirilis di bawah CC0. Anda bebas untuk menyalin, memodifikasi, mendistribusikan, dan menggunakan karya ini untuk tujuan apa pun, termasuk komersial, tanpa meminta izin.

Dukung Maker dengan membeli produk melalui Cetak Biru mereka di mana mereka mendapatkan Komisi Pembuat yang ditetapkan oleh Penjual, atau buat iterasi baru dari Cetak Biru ini dan masukkan sebagai koneksi di milik Anda sendiri.

Diskusi

(0)

Masuk untuk bergabung dengan diskusi

Memuat komentar...